Silicon nitride is used as a diffusion mask, gate material, etch mask interlevel insulator, and passivation overcoat. In all but the latter two applications it is usually present as a thin film, under 100 nm thick.
Silicon oxide is the most common underlayer and in state-of-the-art devices may be about 10 nm thick. I... | text_only | 18_plasma-etching-an-introduction_compress | ||
Nitride films that have been used for some step of device manufacture are often removed prior to further processing without additional masking. This is referred to as a "blanket etch."
## 2. **Etching Methods**
Most forms of silicon nitride can be etched in either barrel or planar plasma or RIE systems. It is most c... | text_only | 18_plasma-etching-an-introduction_compress | ||
## 3. Etching Chemistry Review
Fluorine etchants are the most common for etching silicon nitride. CF 4 and C F 4
+ 0 2 are the most generally employed etchants. Nitrides of nominal composition Si 3 N 4 will usually etch at a rate between that of single crystal Si and Si0 2
. Table 4 summarizes the relative rates of s... | text_only | 18_plasma-etching-an-introduction_compress | ||
## D. Single Crystal Silicon
Numerous applications exist for etching features into single crystal silicon.
Isotropic etching is used to make islands. Trenches of various depths are used in the manufacture of MOS devices. Shallow trenches (0.5 μ to 1.5 μ)
are used to make flat structures (planarization) and to aid i... | text_only | 18_plasma-etching-an-introduction_compress | ||
## 1. Chlorine And Fluorine Etchants
Except at very low pressure, etchants containing only fluorine will etch silicon with at least some isotropic component. Selective oxide etchants usually result in anisotropic silicon profiles as well, but at reduced rates
[26]. Addition of even small concentrations of other halog... | text_only | 18_plasma-etching-an-introduction_compress | ||
Silicon etch rates with chlorine are very sensitive to ion energy, which is reflected by sensitivity to power and frequency [34]. Applying a dc bias to a wafer [35] produces etch rates in excess of 10 microns/minute with a trend for small areas to etch faster than large ones [36]. Usually the higher rates are accompani... | text_only | 18_plasma-etching-an-introduction_compress | ||

## E. Polysilicon
Polycrystalline silicon (Polysilicon) is used primarily for gate electrode material and interconnects. It is also used as an oxidizable source for insulation or, when doped with oxygen, as a passivation layer. It is most often applied to wafers by low pressure che... | text_only | 18_plasma-etching-an-introduction_compress | ||
% Underlayer loss = $\frac{\text{Poly thickness}}{\text{Oxide thickness}}\times\frac{\text{\%over-etch}}{\text{Slectivity}}$
ο For polysilicon 0.3 μ thick over 150 A gate oxide requiring 50% over-etch, a selectivity (based on a single process step) of 30 : 1 is needed. The amount of over-etch necessary is determined by... | text_only | 18_plasma-etching-an-introduction_compress | ||


the ratio of anisotropic to isotropic component in the etch as well as the details of the film profile over the corner. The result is that material displaced from, and parallel to, the edge of the underlying vertical step will etch at a very redu... | text_only | 18_plasma-etching-an-introduction_compress | ||
Polysilicon etch properties depend on doping type and level, the amount of open area (pattern sensitivity) and the concentration of chlorine in the etch gas. With little or no chlorine, doped and undoped material etch very similarly [38]. With increasing chlorine the variation becomes significant.
Heavily phosphorous... | text_only | 18_plasma-etching-an-introduction_compress | ||
There are numerous single, binary, and tertiary mixtures of gases in use for etching polysilicon. Many of them are mixtures of compounds of the form C w H x F y C l z such as C2F5C1. These are often mixed with SF6
. Other common mixtures include the addition of oxygen and/o r hydrogen containing gases. Binary mixtures ... | text_only | 18_plasma-etching-an-introduction_compress | ||
The large number of variables involved in polysilicon etching can make selection of an appropriate process formidable. Some guidance in the form of a trend chart is presented in Fig. 18. Headings are generic, e.g., "Cl 2 "
represents any chlorine containing gas, "passivant," one that is believed to provide side wall p... | text_only | 18_plasma-etching-an-introduction_compress | ||
Many of the chlorine-based etchants that are effective for anisotropic polysilicon etching can be modified for use with suicides. Oxygen can be added to enhance the production of oxychlorides. Oxygen can have a negative effect, however, on dimensional control by enhancing resist erosion.
## G. Aluminu M An D Aluminum... | text_only | 18_plasma-etching-an-introduction_compress | ||
Doped or undoped Si0 2 is the most common underlayer when aluminum is used alone. When used as part of a multilayer metallization a thin layer of titanium, titanium/tungsten or other barrier metal are the most common underlying materials. In some instances a thin layer of these metals may also be used on the top of the... | text_only | 18_plasma-etching-an-introduction_compress | ||
Safety, equipment reliability [44], and preventive maintenance are particularly important in aluminum etching. In the presence of moisture, chlorine residues are readily converted into highly corrosive hydrochloric acid, which rapidly attacks aluminum. This can also lower the reliability of the etched product. Techniqu... | text_only | 18_plasma-etching-an-introduction_compress | ||
The time required to etch through the oxide film is sometimes referred to as the initiation or induction time. Water vapor has a deleterious effect on the removal of the oxide layer. SiCl 4 or BC13 etchants aid in removal of residual water vapor markedly reducing the induction time [48].
3. *Etching the Metal:* Alumi... | text_only | 18_plasma-etching-an-introduction_compress | ||
6. *Resist Removal:* Dry resist removal is most common and is most often a result of Step 5. Sometimes, however, additional cleanup processing may be needed to remove all vestiges of resist. Negative resist, for example, may become so tenacious that ordinary methods are unsuccessful. In this case it is best to consider... | text_only | 18_plasma-etching-an-introduction_compress | ||
Also, **AICI3** can etch aluminum. A possible reaction path that proceeds with the participation of SiCl 4 is,
2A1 + **AICI3** > 3A1C1
```
A1C1 + SiCl 4
> Αία3 + SiCl 2
.
```
Aluminum containing more than trace amounts of copper is one of the more difficult ma... | text_only | 18_plasma-etching-an-introduction_compress | ||
Copper aluminum alloys are even more prone to corrosion after dry etching than pure metal. In part, this is due to the large electronegative potential difference between the two metals; which readily leads to galvanic corrosion. Some form of wet cleanup after etching Cu/A l is highly recommended.
## Vi. Other Materia... | text_only | 18_plasma-etching-an-introduction_compress | ||
When these materials are present, care needs to be taken when using oxygen discharges for cleaning organics. Various additions, such as hydrogen to the gas can surpress the formation of volatile oxides without substantially reducing the cleaning capability.
Chromium is a particularly interesting example of a material... | text_only | 18_plasma-etching-an-introduction_compress | ||

orthogonal designs, for example [54], are readily adapted to cases where more variables need to be considered. Figure 19 displays data points used for a central composite model in three variables. Data so obtained is sufficient to describe the result (say etch rate) over the entire ... | text_only | 18_plasma-etching-an-introduction_compress | ||
## References
[1] George E. P. Box, William G. Hunter, and J. Stuart Hunter, "Statistics for Experimenters," John Wiley & Sons, Inc. New York (1978).
[2] S. N. Deming and S. L. Morgan, *Analytical Chemistry* 45, **278A, March 1973.**
[3] See Chapter 7 by G. K. Herb in this volume.
[4] See Chapters 3 and 4 in this... | text_only | 18_plasma-etching-an-introduction_compress | ||
[15] R. C. Alkire and D. J. Economou, *J. Electrochem. Soc.* 132, 648 (1985).
[16] S. Dushman, J. Lafferty, editor, "Scientific Foundations of Vacuum Technique," 2nd edition, John Wiley & Sons, Inc., New York, (1962).
[17] An excellent compilation of etch gas compositions is given in "The Design of Plasma Etchants,... | text_only | 18_plasma-etching-an-introduction_compress | ||
[23] H. Boyd and M. S. Tang, *Solid State Technology* 22 **(4) 133, April (1979).**
[24] F. Sanders and J. Dielman, H. Peters and H. Sanders / . *Electrochem. Soc.* 129, **2559**
(1982).
[25] D. L. Kendall, "Vertical Etching of Silicon at Very High Aspect Ratios," in Ann. Rev.
Maer. Sci. 9, 373-403, Annual Review... | text_only | 18_plasma-etching-an-introduction_compress | ||
[34] R. Bruce, D. L. Flamm, V. M. Donnelly, and B. S. Duncan, in Extended Abstracts of the Electrochemical Society Fall Meeting, October, St. Louis, MO. Abstract \#243 , Electrochemical Society, Princeton, New Jersey (1981).
[35] V. Ho and T. Sugano, *Thin Solid Films,* 95, **315 (1982).**
[36] R. Bruce and A. Reinb... | text_only | 18_plasma-etching-an-introduction_compress | ||
[47] R. Allen, M. Foster and Y. Yen, *J. Electrochem. Soc.* 129, **1379 (1982).**
[48] K. Tokunaga, F. C. Redeker, D. A. Danner, and D. W. Hess, / . *Electrochem. Soc.* **128,**
851 (1981).
[49] M. Oda and K. Hirata, *Jpn. J. Appl. Phys.* 19, **L405 (1980).**
[50] C. B. Cooper III, M. E. Day, C. Yuen, and M. Salim... | text_only | 18_plasma-etching-an-introduction_compress | ||
[53] G. R. Bryce and D. R. Collette, *Semiconductor International* 71, (1984). [54] D. W. Jillie, P. Freiberger, T. Blaisdell, and J. Mutani, in *Extended Abstracts of the* Electrochemical Society Fall Meeting, October, San Diego, CA. Abstract \#289 . Electrochemical Society, Princeton, New Jersey (1981).
# 6 Ion Bea... | text_only | 18_plasma-etching-an-introduction_compress | ||
## I. Introduction
Ion beam etching is a versatile process for pattern delineation and materials modification. The low pressure, line-of-sight nature of beam techniques provides a flexibility of directional bombardment not available in other plasma processes. Also, the ability to separately control ion energy and flux... | text_only | 18_plasma-etching-an-introduction_compress | ||

are then accelerated through the extraction grid region and travel through the beam plasma region.
Kaufman sources produce several mA/cm 2 ion flux at 500-1000 eV, and are available up to about 30 cm diameter, generating total beam currents exceeding one ampere. At lower energy, t... | text_only | 18_plasma-etching-an-introduction_compress | ||
Together with microwave ion sources, described later, Kaufman sources have the following attributes, which enable highly quantitative etching

processes to be performed:
1. independent control of ion energy and current density, 2. isolation of samples from ion generation process, ... | text_only | 18_plasma-etching-an-introduction_compress | ||
Magnetic Field. To obtain a large number of ions per discharge electron, a magnetic field is applied such that electrons cannot pass directly from the cathode to the anode, but follow helical paths between collisions, greatly increasing their path length and ionization efficiency. The cyclotron radius of a 100 eV elect... | text_only | 18_plasma-etching-an-introduction_compress | ||
Discharge Characteristics. To maintain a glow discharge in the ion source, three conditions must be present: 1. sufficient gas pressure in the discharge chamber, 2. a source of electrons (hot filament),
3. accelerating voltage for electrons (discharge voltage Vd).
To ignite the discharge, the gas pressure is increas... | text_only | 18_plasma-etching-an-introduction_compress | ||
Typical discharge parameters are:
argon pressure = 1 mTorr, ion density = electron density = 10 1 0 /cm3, ion energy in plasma = 0.05 eV,
primary electron energy = 40 eV,
Maxwellian electron energy = 3 eV,
plasma potential = about 5 V above anode potential, discharge voltage = 40 V,
discharge current = 0.2-2.0 A, ... | text_only | 18_plasma-etching-an-introduction_compress | ||
Referring to Fig. 2, to generate an ion beam of 500 eV, a voltage of 500 V
is applied to the anode. The plasma potential is then about 505 V. The accelerator grid is held at a negative potential of about - 50 V relative to ground. Ions are first accelerated by the 555 V potential difference between the plasma and the ... | text_only | 18_plasma-etching-an-introduction_compress | ||
The maximum ion current density that can be extracted from the plasma is space charge limited, and given approximately by:
$$j=K(q/m)^{1/2}V_{t}^{3/2}/I_{g}^{2},$$
,
where j is the maximum current density, Vt is the total potential difference between the grids (Fig. 2), \# is a constant depending on grid geometry, q... | text_only | 18_plasma-etching-an-introduction_compress | ||

in the range 1-2 mm for ion energies up to 1 keV. Current densities over 0.1 mA per aperture at 1000 eV are achieved [6], giving current densities of several mA/cm 2 at the grids, while maintaining low beam divergence half-angles of 5-7 degrees. Molybdenum and graphite are the most ... | text_only | 18_plasma-etching-an-introduction_compress | ||
Effects of Accelerator Grid Potential. Increasing the accelerator grid potential Vacc (Figs. 1, 2) to more negative values enables slightly higher ion currents to be extracted due to increasing Vt
. Since the accelerate-decelerate sequence of the extraction grid region acts as a defocusing lens, however, increasing Vac... | text_only | 18_plasma-etching-an-introduction_compress | ||
## 3. Beam Plasma Region
Beam Plasma Characteristics. In the beam region the ion current density is typically high enough that electrostatic repulsion between ions alone (space charge) would sharply fan out the beam once it left the extraction region.
This space charge repulsion is prevented by the presence of an eq... | text_only | 18_plasma-etching-an-introduction_compress | ||
Neutralization. If the ion beam strikes a conducting grounded surface, enough secondary electrons are generated to balance the space charge of the beam, and external neutralization is not necessary. If the ion beam strikes an insulating surface, however, with no external source of electrons, the insulator surface charg... | text_only | 18_plasma-etching-an-introduction_compress | ||

# Ion-Neutral Interactions

Ion energy is determined by the anode potential and is usually assumed to be within 5-10 eV of this value. The actual ion energy can be measured with a retarding grid analyzer (Fig. 5). This analyzer can separately mea... | text_only | 18_plasma-etching-an-introduction_compress | ||
RESONANT CHARGE

DIRECTED MOMENTUM
LOSS COLLISION
product of mean-free-path and pressure. This quantity is given for argon in Fig. 6 for both collisions as a function of ion energy. As an example, for 500 eV argon ions traveling through a background pressure of 0.1 mTorr, the dir... | text_only | 18_plasma-etching-an-introduction_compress | ||
The cross section for resonant charge exchange is much larger than the cross section for directed momentum loss, and the mean-free-path is


correspondingly shorter. For 500 eV argon ions in 0 1 mTorr argon (Fig. 6),
the mean free path is 1.2 m.... | text_only | 18_plasma-etching-an-introduction_compress | ||
## B. Microwave Ion Sources
Microwave ion sources, also called electron cyclotron resonance (ECR) sources, have been applied to reactive ion beam etching in the past several years [11], and also to plasma deposition. They share many basic features with the Kaufman source. Ions are produced by electron bombardment in a... | text_only | 18_plasma-etching-an-introduction_compress | ||

region. This shield acts as a microwave reflector, and also improves the region of voltage that is stable against sparkover. Additional characterization of such a microwave plasma is given by Keqiang *et al.* [13]. The considerations of beam divergence, flux measurement and neutrali... | text_only | 18_plasma-etching-an-introduction_compress | ||
## A. Sputtering Yields An D Etch Rates
In the ion energy range of tens of eV to several keV, the sputtering yield
(number of sputtered atoms per incident ion) increases nearly linearly with ion energy. A detailed compilation of sputtering yields of different beam and target species is given by Matsunami *et al.* [15... | text_only | 18_plasma-etching-an-introduction_compress | ||
The angular dependence of etch rates (or sputtering yields) is not commonly measured or published for many materials, yet it strongly affects the resulting shapes of etched surfaces that contain topographic structure.

The typical dependence of sputtering yield on the angle of ion ... | text_only | 18_plasma-etching-an-introduction_compress | ||
In order to accurately transfer a pattern from mask to substrate, the mask shape must be controlled. For example, if the mask edges are sloped (Fig. 10a), the edge of the etched step advances sideways during etching,

leading to sloping edges in the final substrate pattern. Another... | text_only | 18_plasma-etching-an-introduction_compress | ||
Optimization of tilt angles for various mask/substrate combinations depends on the angular dependence of the sputtering yields (as in Fig. 9), and is thoroughly discussed by Lee [18].
## C. Limits O F Etching Resolution
The highest resolution structures obtained by ion beam etching have been

This principle of reducing the etch rate to near zero by a combination of low ion energy and added oxygen was used by Kinoshita *et al.* [24] to gain a selectivity of 13 in etching GaAs relative to Al 0 5 G a 0 5 A s . As shown in Fig.
17, using 2% 0 2 in Ar, there is little selec... | text_only | 18_plasma-etching-an-introduction_compress | ||
Few examples have been published using nitrogen/argon mixtures to obtain preferential etch rates, but a similar degree of selectivity should be achieved with nitrides as with oxides. There is an equivalent range of reactivity of nitrides as with oxides, with many materials used in microelectronics having stable nitride... | text_only | 18_plasma-etching-an-introduction_compress | ||
Norma l operation is easily restored by cleaning the anode.
Etching of Si and Si0 2 is accomplished by fluorocarbon and chlorocarbon gases, or chlorine, usually in a mixture with argon to minimize the effect on the filament cathode [26]. With these gases, a microwave ion source has the advantage of a filament-free di... | text_only | 18_plasma-etching-an-introduction_compress | ||
Mass analysis of similar beams by Mayer and Barker [29] shows that the primary ion constituent is CF3
+
with low plasma densities in the source, but that the beam composition is a strong function of the plasma conditions.
The asterisk in Fig. 19 indicates the maximum etch rate achievable with C F 3
+
ions alone. ... | text_only | 18_plasma-etching-an-introduction_compress | ||
## C. Ion-Assisted Chemical Etching
The addition of a chemically reactive gas (e.g., Cl 2 ) to the substrate region of an argon ion beam system is generally referred to as ion-assisted chemical etching, to distinguish it from the case where the reactive gas is introduced through the ion source. The distinction is not ... | text_only | 18_plasma-etching-an-introduction_compress | ||
The effect of added Cl 2 on the argon ion etch rate of Si is shown in Fig.
20 [30]. The sputtering yield curve is displaced upwards by increasing the flow of CI 2 , to the point where the effective etch yield rises by a factor of 3 or more. GaAs is commonly etched by Cl-containing gases, often using the directionalit... | text_only | 18_plasma-etching-an-introduction_compress | ||

## V. Ion Etching Combined With Growth Or Deposition A. Surface Compound Layer Formation
Although this article is mainly concerned with etching applications where material removal is the objective, ion etching also induces the formation of a surface compound layer in some cases. On... | text_only | 18_plasma-etching-an-introduction_compress | ||

combinations may require dilution of the gas and higher ion beam energies to achieve this balance [34]. Silicon oxidation and nitridation, performed under net etching conditions, show promising electrical properties as measured by MOS capacitor and transistor structures [35].
## B... | text_only | 18_plasma-etching-an-introduction_compress | ||
Preferential resputtering of film components can cause film composition to differ markedly from the target composition [17, 40]. Similarly, ion bombardment by oxygen or nitrogen during metal deposition can produce selective oxide or nitride phase formation [41, 42]. The effect of nitrogen ion bombardment on the deposit... | text_only | 18_plasma-etching-an-introduction_compress | ||
Clearly, the similarity between ion etching processes and ion modification processes during thin film growth gives much information of use in both areas of application. Ion beam studies will continue to provide insight into the mechanisms of plasma processes, and the advantages of low pressure, directed bombardment wil... | text_only | 18_plasma-etching-an-introduction_compress | ||
J. M. E. Harper, J. J. Cuomo, and H. R. Kaufman, / . *Vac. Sci. Technol.* **21, 737 (1982).**
R. S. Robinson, NASA-CR-159567 (1979).
R. J. Warmack, J. A. D. Stockdale, and R. N. Compton, Int. J. Mass Spectrometry and Ion Physics **27, 239 (1978).**
R. S. Robinson, *J. Vac. Sci. Technol.* **16, 185 (1979).**
S. Mat... | text_only | 18_plasma-etching-an-introduction_compress | ||
Bresnock, / . *Electrochem. Soc.* **128, 1077 (1981).**
J. W. Coburn and H. F. Winters, / . *Vac. Sci. Technol.* 16, 391 (1979).
T. M. Mayer and R. A. Barker, / . *Electrochem. Soc.* **129, 585 (1982).**
J. D. Chinn, W. Phillips, I. Adesida, and E. D. Wolf, / . *Electrochem. Soc.* **131, 375**
(1984).
S. Matsui,... | text_only | 18_plasma-etching-an-introduction_compress | ||
| I. Legislated Safety Obligations | 426 |
|------------------------------------------------------------------------------------------|-------|
| A. Federal Legislation | 426 |
| B. State Legisl... | text_only | 18_plasma-etching-an-introduction_compress | ||
| E. Flammability | 440 |
| F. Chemical Toxicity | 440 |
| G. Impurities in Gas Sources | 442 |
| V. Hazardous Ga... | text_only | 18_plasma-etching-an-introduction_compress | ||
ISBN 0-12-469370-9 The basic characteristic that is exploited in plasma processing is the ability of the process to achieve anisotropic pattern transfer for device designs that have aspect ratios (feature dimension/film thickness) less than three. This necessarily demands that the plasma process use feed gases that are... | text_only | 18_plasma-etching-an-introduction_compress | ||
## I. Legislated Safety Obligations
So that we can perform our work safely, however, we must be adequately informed about our legislated obligations. A good source for this information is often your local company safety representative, or the local state or federal OSHA (Occupational Safety and Health Agency) or EPA (... | text_only | 18_plasma-etching-an-introduction_compress | ||
Interpretations of the law are often necessary because of the sweeping OSHA guideline. Any new or novel case is usually dealt with on an individual basis. By the practice of the best-known and identified safety procedures, the best response to any legislated responsibilities is provided.
An even more sweeping legisla... | text_only | 18_plasma-etching-an-introduction_compress | ||
Resource Conservation and Recovery Act (45CFR12.272-12-746 in 1976)
[6, 7] tracks hazardous waste in storage, transport, and disposal.
The Department of Transportation regulates the transport of all compressed gases and the methods of containment of these gases [8].
N o t all federal agencies are regulatory. There... | text_only | 18_plasma-etching-an-introduction_compress | ||
## B. State Legislation
During the Reagan Administration, there has been an attempt to shift the responsibility of regulating the workplace and the environment from federal to state jurisdiction. The states have enacted legislation that has become known as the "sunshine laws" or the "right-to-know laws." Basic to thes... | text_only | 18_plasma-etching-an-introduction_compress | ||
New Jersey requires *all* companies to update this workplace list annually and to send copies to state and county health departments and local fire and police groups. The environmental list must also be annually given to state officials, county officials, and local health, fire, and police departments. There are no cor... | text_only | 18_plasma-etching-an-introduction_compress | ||
Unde r the federal mandate, chemical manufacturers, importers, and distributors must comply to the law. All other manufacturers must retain the fact sheet if they buy hazardous chemicals, while there is no need for nonusers of hazardous substances to comply. In New Jersey *all* manufacturers, hospitals, wholesalers, cl... | text_only | 18_plasma-etching-an-introduction_compress | ||
The general conclusion of this state study was that the semiconductor industry has not ignored the consequences of hazardous chemicals and, in general, has established adequate state-of-the-art safety procedures that comply with the legislation. Some of the conclusions of this study are [10]:
- that of the facilities ... | text_only | 18_plasma-etching-an-introduction_compress | ||
This Cal/DIR-DOS H study presented a good review of four major areas of interest. Each of these four areas was documented with respect to the general procedure and activities that are necessary to result in four products; silicon wafers, silicon devices, GaAs wafers, and GaAs devices. The production of both silicon and... | text_only | 18_plasma-etching-an-introduction_compress | ||
The equipment designers and builders have long been aware that the methods used in the semiconductor industry have seemingly incorporated some of the worst hazards from many other industries, including:
- high temperatures (up to 1200°C),
- high voltages (up to 400 kV),
- x-rays,
- laser radiation, UV radiation,
-... | text_only | 18_plasma-etching-an-introduction_compress | ||
Because the designers and builders recognized that safer apparatus must be available, equipment design must expect normal usage conditions, and there is a duty to instruct and warn about safety, the Semiconductor Equipment Manufacturers Institute began in 1973 [11]. This is an organization that recognizes that a cooper... | text_only | 18_plasma-etching-an-introduction_compress | ||
If money is not the total solution, what is? There is a general acceptance of the concept that "If you want to get somewhere, you had better know where you are." This old saw holds excellent advice for a proper strategy for determining the best response to the requirements that are placed on us for safety and health re... | text_only | 18_plasma-etching-an-introduction_compress | ||
The proper identification of the risk status will determine if the cost is too high. For an installation of capital-cost equipment into the semiconductor facility, AT& T Bell Laboratories has determined that an additional 20-30 percent of the cost must be added to the purchase price to provide for safety.
A strong co... | text_only | 18_plasma-etching-an-introduction_compress | ||
The interplay between the elements of risk-cost-safety cannot be overstated. Understanding the degree of risk and the necessary changes to guarantee an operation with total regard for safety will allow the cost to be properly defined to management for their enthusiastic support. Being informed of the necessary actions ... | text_only | 18_plasma-etching-an-introduction_compress | ||
## A. Plasma Feed Gas Source
Almost without exception the plasma feed gas(es) are contained in a compressed gas cylinder. It is of utmost importance that knowledge be available about the physical state of the contents of the cylinder (gas or liquid) and the chemical consequences and hazards of the cylinder contents.
... | text_only | 18_plasma-etching-an-introduction_compress | ||
The Department of Transportation Office of Hazardous Materials Operations has its regulations published primarily in CFR 49 [8]. DOT controls the shipment of hazardous materials (including all compressed gases) by all common carriers. It requires proper shipping containers, acceptable shipping papers, shipper certifica... | text_only | 18_plasma-etching-an-introduction_compress | ||
The DO T labeling scheme is similar to the ANSI standards and also conforms to the United Nations' eight hazardous material groupings. These groups include:
1. Explosives. Three subdivisions include those materials that are capable of detonation with a moderate spark, shock, or flame, and propagating the explosion to ... | text_only | 18_plasma-etching-an-introduction_compress | ||
5. Poisons. Three classes: Class A poisons are life threatening with a small amount of gas or vapor (POISON GAS—cyanogen, arsine, phosphine, fluorine); Class Β poisons are life threatening by contacting or ingesting the liquid or solid material (POISON—nitric acid, sodium cyanide, lead, and arsenic salts); and Class C ... | text_only | 18_plasma-etching-an-introduction_compress | ||
9. Biomedical material. Any material that may cause disease (BIOMEDICAL MATERIAL).
10. Required notice on some transport vehicles (EMPTY).
11. Special notice. Required when freight contains two or more classified materials or 5000 lbs. or more of classified materials are loaded on the vehicle (DANGEROUS).
12. Chl... | text_only | 18_plasma-etching-an-introduction_compress | ||
## Iv. Characteristics Of **Cylinder Gases** A. Cylinder Pressure
The gases that are included in this group are those that have cylinder pressure greater that 500 psig at 70°F. Some of these are Ar, CF 4
, He, H 2
,
N 2
, 0 2
, SiH4
, and SiF4
. Typically the delivery pressure for the costly autoflow systems of many ... | text_only | 18_plasma-etching-an-introduction_compress | ||
Another aspect of controlling the delivery gas pressure to a low value
( < 20 psig) is that in many installations the gas cylinder may be a considerable distance from the use point (plasma reactor). Here the gas pressure should be kept low in the lengthy delivery line so that if a leak occurs, the escaping gas has low... | text_only | 18_plasma-etching-an-introduction_compress | ||
| He | (gas) | 96.7 ft 3 / l b |
|-------|----------|-------------------|
| N H 3 | (liquid) | 22.6 |
| SiH4 | (gas) | 12.1 |
| o2 | (gas) | 12.1 |
| P H 3 | (liquid) | 11.4 |
| HC1 | (liquid) | 10.9 |
For those materials that have hi... | text_only | 18_plasma-etching-an-introduction_compress | ||
The cylinder size is also important if a decision is made to contain the total volume of escaped gas within the gas cabinet if an accident occurs to minimize the contaminated area. The specific volume then determines what the required exhaust speed must be so that no hazardous material escapes the gas cabinet.
## C. ... | text_only | 18_plasma-etching-an-introduction_compress | ||
## D. Corrosiveness
The main corrosive materials that are commonly used as feed source gases for plasma processes are BC13
, SiCl 4 and C1F3
. The selection of a suitable gas pressure regulator with a diaphragm material that will not rapidly be digested by the corrosive is of utmost importance. The material compositio... | text_only | 18_plasma-etching-an-introduction_compress | ||
## E. Flammability
The flammability of various materials that are used in plasma operations, along with the flammable limits in air, are given next [19].
| SiH4 | spontaneously |
|---------|-----------------|
| P H 3 | spontaneously |
| C 3 H g | 2.2-9.5% in air |
| H 2 | 4-75% in air |
| CO | 1... | text_only | 18_plasma-etching-an-introduction_compress | ||
Any chemical is classified as a toxic chemical that when ingested, inhaled, or absorbed, or when applied to, injected into, or developed with the body, in small amounts, by its chemical action may cause damage to structure or disturbance to bodily function [21, 22]. The bodily damage can be local (confined to exposed a... | text_only | 18_plasma-etching-an-introduction_compress | ||
The hazardous concentrations are usually given in ppm (parts toxic chemical concentration per million parts nontoxic medium) and g/K g (the weight of the toxic substance per kilogram weight of "average" human). Some commonly used chemicals in plasma processing and their PEL and IDLH
values (ppm) are given next [19, 24... | text_only | 18_plasma-etching-an-introduction_compress | ||
As the toxic level of a chemical that is used in a process increases, the smaller should be the amount of the chemical that should be stored at any source location for the process system. This practice is also good procedure for even the storage of such materials in a central holding, or "gas house" area. The less of t... | text_only | 18_plasma-etching-an-introduction_compress | ||
The incorporation of phosgene and carbon dioxide in boron trichloride is a result of the chemistry used to make BC13
:
4BO + 3C 4- 8C12
-* 4BC13
+ 2COCl 2
+ C0 2
, and 3B4C 4- 202
+ 20C12
-> 12BC13
+ 2C0C1 2
+ C0 2
.
The impurity level of COCl 2 in BC13 from the manufacturer is high, 800-1000 ppm. After filt... | text_only | 18_plasma-etching-an-introduction_compress | ||
## V. Hazardous Gas Monitoring Instruments
Being able to warn the workforce about the presence of dangerous concentrations of hazardous and toxic materials is a primary function of a working safety program. The identification of the proper instrumentation that serve this significant purpose is important. The propertie... | text_only | 18_plasma-etching-an-introduction_compress | ||
IDLH, LC 5 0 **and nose irritation**
| AMMONIA | PHOSGENE | |
|----------------------------------------------------------|-----------------------------------------------------------... | text_only | 18_plasma-etching-an-introduction_compress | ||
trations. On the other hand, the nose does not become irritated to the presence of phosgene until the gas concentration is 100 times the PEL
value! Even at 5 times the IDLH concentration, the nose just becomes irritated to phosgene, at which time it will most undoubtedly be too late.
The nose can be relied on to pro... | text_only | 18_plasma-etching-an-introduction_compress | ||
The nose can be relied on to provide good information about the presence of some hazardous chemicals, but the possible desensitivity with time and those chemicals that cannot be detected are important data to be known and continually reviewed.
There is another effect from hazardous chemicals that must be understood s... | text_only | 18_plasma-etching-an-introduction_compress | ||
## Vi. **Checking The Workplace For Hazardous Chemicals**
If there is any reason that a check be made of the work environment, perhaps because of a "strange smell," a complete chemical analysis must be made to ensure that no hazardous condition exists. Remember that the
"sunshine laws" guarantee that the worker has t... | text_only | 18_plasma-etching-an-introduction_compress | ||
NIOSH suggests that another concentration level be considered, the allowed level (AL), that is, perhaps one-tenth of the PEL level. This AL will then provide more than adequate warning potential before PEL is reached.
Appendix Β lists 45 common gas and liquid sources for many plasma etch chemistries used in microelec... | text_only | 18_plasma-etching-an-introduction_compress | ||
Early in the development of the CC1 4 aluminum etch process, it was observed that a strong medicinal odor was generated when the reactor was wiped with Kim Wipes dipped in warm DI water. The cleaning procedure removed all traces of the film, and an oxygen plasma was used to dry the reactor before the aluminum etch was ... | text_only | 18_plasma-etching-an-introduction_compress |
Subsets and Splits
No community queries yet
The top public SQL queries from the community will appear here once available.