title: Process-map conventions for polymer SLS (PA12)
|
| 3 |
+
summary: Canonical axes (Andrew number, VED, EMR), the two process windows (bed-temperature sintering window vs stable sintering region), property-vs-energy curve shape, and the published precedent for percent-based relative energy axes on desktop machines.
|
| 4 |
+
---
|
| 5 |
+
|
| 6 |
+
> **DRAFT — PENDING HUMAN REVIEW.** Synthesized from a 2026-07-26 literature
|
| 7 |
+
> pass (primary-source verified where noted, incl. both Vasquez papers and
|
| 8 |
+
> Bourell CIRP 2017 read in full). Grounds the dashboard Process Map page.
|
| 9 |
+
|
| 10 |
+
# Process maps for polymer SLS of PA12
|
| 11 |
+
|
| 12 |
+
## Canonical axes
|
| 13 |
+
|
| 14 |
+
Published PA12 parameter studies vary laser power P [W] as the primary knob
|
| 15 |
+
(scan speed v, hatch h, layer t, beam size held constant — Bourell 2017);
|
| 16 |
+
part-bed temperature is treated as a *window constraint*, not a map axis.
|
| 17 |
+
Derived quantities:
|
| 18 |
+
|
| 19 |
+
- **Andrew number (areal ED)**: A_N = P/(v·h) [J/mm²]. Defined from the
|
| 20 |
+
start as a *relative* measure (Nelson 1993; Williams & Deckard, SFF 1996).
|
| 21 |
+
PA12 working range ~0.01–0.04 J/mm² (Bourell 2017); optima are
|
| 22 |
+
machine/powder-specific (one Formiga study: 0.048–0.067 J/mm²) — do not
|
| 23 |
+
hard-code a single number. Omits layer thickness.
|
| 24 |
+
- **Volumetric ED**: E_v = P/(v·h·t) [J/mm³]. Collapses layer-thickness
|
| 25 |
+
variation. PA12 anchors (Bourell 2017): density knee ~0.12 J/mm³; UTS
|
| 26 |
+
peaks 51 MPa, declines to ~47 MPa above ~0.3 J/mm³. PA12/CF optimum
|
| 27 |
+
0.23–0.24 J/mm³ (Lupone 2021). Typical optimum band ~0.2–0.35 J/mm³.
|
| 28 |
+
⚠ VED conventions differ across papers — match the formula before comparing.
|
| 29 |
+
- **Energy Melt Ratio**: EMR = applied VED ÷ E_m, where
|
| 30 |
+
E_m = [C_p·(T_m − T_bed) + h_f]·ρ·φ (Starr, Gornet & Usher 2011 — NOT
|
| 31 |
+
"Starr/Rios/Fulcher"; that citation circulating in older notes is wrong).
|
| 32 |
+
The literature's accepted cross-machine / cross-bed-temperature
|
| 33 |
+
normalizer. PA12 on the Vasquez 2013 convention (EOS P100, bed 172 °C,
|
| 34 |
+
φ≈0.5): E_m = 0.069 J/mm³, E_deg = 0.43 J/mm³, degradation at EMR ≈ 6.2,
|
| 35 |
+
practical optimum EMR ≈ 4–5 (Lupone 2021). ⚠ "EMR ≈ 1–3" folklore is not
|
| 36 |
+
supported on this convention. Bierwisch 2021 extends to AMR (optical
|
| 37 |
+
absorption correction) — relevant for blue diodes on white PA12.
|
| 38 |
+
|
| 39 |
+
## Two distinct process windows (don't conflate)
|
| 40 |
+
|
| 41 |
+
1. **Bed-temperature sintering window** (Goodridge 2012 / Schmid 2014):
|
| 42 |
+
T_bed between crystallization onset and melt onset. PA12: T_m 184.8 °C,
|
| 43 |
+
T_c,peak 146.5 °C, window ≈ 27.6 °C wide, typical setpoint ≈ 168 °C.
|
| 44 |
+
Too low → curl/warp/delamination; too high → caking.
|
| 45 |
+
2. **Stable sintering region** on the laser-energy axis (Vasquez 2011/2013):
|
| 46 |
+
floor = full particle melt (E_m), ceiling = degradation onset (TGA 1 %
|
| 47 |
+
mass loss 322–325 °C; laser can drive local powder >300 °C). Regions:
|
| 48 |
+
unsintered (EMR <~1) → rising properties (1–4) → stable optimum (4–5) →
|
| 49 |
+
degradation (≳6.2: chain scission, gas porosity, orange peel, Bonus-Z
|
| 50 |
+
growth, property decline). Raising T_bed lowers E_m and shifts the whole
|
| 51 |
+
usable band down — exactly what EMR normalizes. No keyhole regime in
|
| 52 |
+
polymer SLS; balling is marginal, not a canonical region.
|
| 53 |
+
|
| 54 |
+
## Property-vs-energy overlay
|
| 55 |
+
|
| 56 |
+
Universal shape: rise → plateau → decline. Strength/modulus plateau first;
|
| 57 |
+
**elongation-at-break keeps rising to higher EMR and is the most
|
| 58 |
+
energy-sensitive property** (Starr 2011) — best single process-health
|
| 59 |
+
indicator. Anchors: Vasquez 2013 peak UTS 53.9 MPa at 18 W, −3.5 % at
|
| 60 |
+
22–25 W; EOS PA2200 datasheet UTS 45±3 MPa, modulus 1700±150 MPa,
|
| 61 |
+
elongation 20±5 % X/Y (Z 4–9 %). Desktop diodes (Sinterit Lisa 5 W:
|
| 62 |
+
UTS 45–48 MPa but elongation 2–6 %) sit on the rising flank.
|
| 63 |
+
|
| 64 |
+
## Relative (percent) energy axes are publishable practice
|
| 65 |
+
|
| 66 |
+
Sinterit Lisa exposes only a "Laser Power Ratio" multiplier; peer-reviewed
|
| 67 |
+
studies (Olejarczyk 2020, Gharate 2023, Joch 2025) report the relative
|
| 68 |
+
setting as the energy axis directly. Stronger option: one-time optical
|
| 69 |
+
power-meter calibration of % → W (would exceed the literature standard for
|
| 70 |
+
desktop SLS), then compute A_N/EMR physically.
|
| 71 |
+
|
| 72 |
+
## Inova MK1 specifics
|
| 73 |
+
|
| 74 |
+
- Firmware `LaserFillEnergyDensity` is **linear** ED (mJ per mm of scan
|
| 75 |
+
path ≈ P/v), globally scaled by `TotalEnergyDensityPercent`. Divide by
|
| 76 |
+
hatch spacing to get A_N; by hatch × layer for VED. Spot ~250–350 µm
|
| 77 |
+
(hackaday/sls4all sources, unverified); hatch = spot × (1 −
|
| 78 |
+
HotspotOverlapPercent/100).
|
| 79 |
+
- Laser: 5 W optical (dev) / 10 W (production), 445–450 nm, PWM control.
|
| 80 |
+
- At 445 nm neat white PA12 absorbs poorly (Gueche 2021) — absolute
|
| 81 |
+
absorbed energy is uncertain, which itself argues for the relative /
|
| 82 |
+
EMR-band presentation.
|
| 83 |
+
|
| 84 |
+
## Recommended map views (dashboard)
|
| 85 |
+
|
| 86 |
+
1. EMR-normalized energy strip with property overlay + literature bands
|
| 87 |
+
(needs DSC params + bed setpoint + calibrated watts).
|
| 88 |
+
2. P–v (or relative-ED) plane with iso-A_N contours, points colored by
|
| 89 |
+
outcome — implemented as the Process Map page's Map view using
|
| 90 |
+
EffectiveLineEnergyDensity.
|
| 91 |
+
3. Bed-temperature window strip (146.5 / 168 / 184.8 °C) — companion, kept
|
| 92 |
+
separate from the energy views.
|
| 93 |
+
|
| 94 |
+
Full citation list (33 refs incl. DOIs): see the 2026-07-26 research
|
| 95 |
+
transcript; load-bearing ones: Nelson 1993; Williams & Deckard SFF 1996 /
|
| 96 |
+
RPJ 1998; Starr RPJ 17(6) 2011 doi:10.1108/13552541111184143; Vasquez
|
| 97 |
+
Proc IMechE B 2011 doi:10.1177/0954405411414994; Vasquez Polym Eng Sci
|
| 98 |
+
2013 doi:10.1002/pen.23386; Bourell CIRP Annals 66 (2017)
|
| 99 |
+
doi:10.1016/j.cirp.2017.04.128; Lupone eXPRESS Polym Lett 2021
|
| 100 |
+
doi:10.3144/expresspolymlett.2021.16; Han Int J Extreme Manuf 2022
|
| 101 |
+
doi:10.1088/2631-7990/ac9096; Olejarczyk Appl Sci 2020
|
| 102 |
+
doi:10.3390/app10186184; Bierwisch Mater Des 2021
|
| 103 |
+
doi:10.1016/j.matdes.2020.109432; Sommer Polymers 2024
|
| 104 |
+
doi:10.3390/polym16101366.
|
| 105 |
+
|
| 106 |
+
## Discrepancies with existing drafts
|
| 107 |
+
|
| 108 |
+
- `energy-density-cheatsheet.md` quotes "PA12 AED ≈ 0.02–0.1 J/mm²"; the
|
| 109 |
+
verified Bourell 2017 dataset spans ~0.005–0.04 J/mm² with secondary
|
| 110 |
+
sources at 0.02–0.035. Reconcile before promoting either draft.
|
| 111 |
+
- Any note citing "Starr/Rios/Fulcher" for EMR should be corrected to
|
| 112 |
+
Starr/Gornet/Usher (RPJ 2011).
|