| through-the-wall tools ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| vacuum drying ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| vapor cleaning ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| vapor phase HF ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| Verwey-Overbeek theory ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| wafer back surface ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| - ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| wafer cleaning ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
| wafer surface particle detection ... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
wet cleaning 255,256,437,474,482, 566,574
- equipment 443 wet oxidation 306 wet station 12, 34, 39 X-ray micro analysis 251 X-ray photoelectron spectrometry 567 X-ray photoelectron spectroscopy 174,179,449 XMA 251 XPS 174, 179,449,567, 577 XPS spectra 546,547 yield 34
- prediction curves 6 yield-reduction factors 5 z... | text_only | 14_Ultraclean Surface Processing of Silicon Wafers | ||
Kazuo Nojiri Dry Etching
 Technology for Semiconductors Dry Etching Technology for Semiconductors Translation supervised by Kazuo Nojiri Translation by Yuki Ikezi
Kazuo Nojiri Dry Etching Technology | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
 for Semiconductors Kazuo Nojiri Lam Research Co., Ltd. Tokyo , Japan Based on translation from the Japanese language edition: HAJIMETE NO HANDOTAI DRY ETCHING GIJUTSU by Kazuo Nojiri Copyright © 2012 Kazuo Nojiri All rights reserved. ISBN 978-3-319-10294-8 ISBN 978-3-319-10295-5 (eBook) ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
RightsLink at the Copyright Clearance Center. Violations are liable to prosecution under the respective Copyright Law. The use of general descriptive names, registered names, trademarks, service marks, etc. in this publication does not imply, even in the absence of a specifi c statement, that such names are exempt from... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
# Pref Ace
Dry etching is a key technology comparable in importance to lithography as a means for scaling and enhancing the integration level of semiconductor devices. The number of engineers engaged in dry etching development is also comparable to those working on lithography. Lithography technology is relatively ea... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Dry etching technology may sometimes be eclipsed by lithography, but, as already mentioned, it is a key technology that is just as critical as lithography. By way of example, in dry etching, (1) specifi c equipment and process technologies are used for each material, such as Si, SiO 2 , and metal; (2) new technologies ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The book is designed not only to help readers understand the fundamentals of dry etching but also gain a more practical knowledge. The author hopes to provide a guiding principle for engineers who pursue dry etching development. Tokyo, Japan Kazuo Nojiri October 2014
# English Tr Anslation
Translation supervised by ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| 1 | The Contribution of Dry Etching Technology to Progress in Semiconductor Integrated Circuits | 1 |
|------------|-------------------------------------------------------------------------------------------------|-----|
| 1.1 | Dry Etching Overview ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| 2.2.1 | Ion Sheath and Vdc | 16 |
| 2.2.2 | Ion Scattering in the Sheath | 18 |
| 2.3 | How to Design Dry Etching Processes ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| 3.1.1 | Poly–Si Gate Etching | 32 |
| 3.1.2 | Across-Wafer Critical Dimension Uniformity Control | 33 |
| 3.1.3 | WSi2/Poly–Si Gate Etching ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| Contents | | |
|------------|---------------------------------------------------------------------------|-----|
| 3.2 | Silicon Dioxide Etching | 39 |
| 3.2.1 | Mechanism of S... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| 4.1 | History of Dry Etching Equipment | 57 |
| 4.2 | Barrel-Type Plasma Etcher | 59 |
| 4.3 | Capacitively Coupled Plasma Etcher | 60 |
| 4.4 | Magnetron Reac... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| 5.2.2 | Mechanism of Wafer Charging | 78 |
| 5.2.3 | Evaluation and Reduction of Charging Damage for Various Types of Etchers | 81 |
| 5.2.4 | Pattern-Dependent Gate Oxide Breakdown | 87 |
| References | 89 ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
x
| 7 | Future Challenges and Outlook for Dry Etching Technology | 113 |
|------------|-------------------------------------------------------------|-------|
| 7.1 | Innovations in Dry Etching History | 113 |
| 7.2 | Future Challenges and Outlook ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
A higher LSI device density means that there are a larger number of devices built into each chip, and the key is to make each device as small as possible. The fundamental technology for realizing this is fi ne geometry processing, which is mainly comprised of the lithography and dry etching technologies. Lithography is... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


Fig. 1.3 LSI chips formed on a wafer

wafer diameters are indispensable in the semiconductor business. Technology innovations in dry etching are needed to achieve both.
## 1.1 Dry Etching Overview
Figure 1.4 s... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Figure 1.5 shows a dry etching process fl ow. A gate etching process is shown as an example; the steps involved in this process follow: 1. A gate oxide fi lm is fi rst formed on Si substrate. Then poly–Si, which is the gate material, is deposited on top.
2. Next, gate patterns are formed on a resist mask by lithograp... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
A ratio of etch rates (ER1/ER2) between the etch target fi lm and the underlying fi lm and a ratio of etch rates (ER1/ER3) between the etch target fi lm and the mask are called the selectivity to the underlying fi lm and the selectivity to the mask, respectively. These are parameters that indicate how much the underlyi... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Therefore, etching with better uniformity increasingly becomes necessary. MOS transistors are discussed in more detail in the next section.

Parameters for evaluation 1. Etch rate : Etch target film (ER1), Underlying film (ER2), Mask (ER3)
2. Selectivity : Etch target film/Underlying... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


"1" or "0," depending on whether or not the capacitor is charged, respectively. Figure 1.9 shows a manufacturing process fl ow for DRAM. Details of the process fl ow are as follows: 1. The DRAM manufacturing process starts from a bare Si substrate. 2... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

6. After an interlayer insulating fi lm is deposited, contact holes to the Si substrate are opened by self-aligned contact (SAC) etching. Since the gates are covered with an Si 3 N 4 fi lm, which is an etch stop layer, the contact holes and the gate would not be shorted even when the... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
9. The cells are fi lled with a capacitor lower electrode (normally poly–Si), a capacitor insulating fi lm, and a capacitor upper electrode (normally TiN), and the capacitors are thus formed.
10. After an interlayer insulating fi lm is deposited, via holes for connecting the capacitors and metal lines are etched.
... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
In the discussion on the fundamentals of plasma, all the topics for understanding dry etching mechanisms are covered, including "What is a plasma?", the plasma parameters, and the collisions and reactions that take place in the plasma.
Then there is a discussion on the behaviors of ions, which play an important role i... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


Electron expelled from outermost shell Fig. 2.2 Principle of gas discharge

within the plasma, it has a conductive property. When a radiofrequency (RF) power is applied on a pair of electrodes in an etch chamber, el... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The plasma is classified into a completely ionized plasma, in which 100% of electrons and ions are ionized, and a weakly ionized plasma, in which the degree of ionization is low and a mixture of ions, electrons, and neutral atoms and molecules coexist. A glow discharge is used for dry etching. A plasma generated by the... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
$${\frac{1}{2}}m_{c}\nu_{c}^{2}={\frac{3}{2}}k T_{c}$$
$$(2.1)$$
2 m k e e n = Te (2.1)
where me is the electron mass, νe is the electron velocity, and k is Boltzmann's constant.
| Gas temperature Tg (K) | | | | | |
|--------------... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Because electrons are very light, they are accelerated by the electrical field and acquire a large kinetic energy. The average electron energy in a glow discharge plasma is several electron-volts. Say the electron energy is 2 eV; then the electron temperature Te is 23,200 K, according to Eq. (2.1). On the other hand, t... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 2.1.3 Collision Processes In A Plasma
Electrons that have gained energy in a plasma collide with atoms and molecules.
These collisions are categorized as elastic collisions and inelastic collisions.
Figure 2.4 summarizes the collision processes in a plasma. With an elastic collision, only the kinetic energy cha... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
2. Ionization: As mentioned earlier, an electron in the outermost shell is expelled when the energy of the colliding electron is larger than the ionization voltage, and the neutral atom turns into a positive ion. This reaction step is described as follows:
## A+E→A+ +2E
3. Dissociation: Dissociation occurs when the e... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
As a result, only the electrons accelerated by the electric field jump into the electrodes. Because the lower electrode is connected to a blocking capacitor, it is gradually biased to a negative potential. A direct current (DC) bias that is thus generated is referred to as a self-bias and is represented by Vdc. While t... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Electrons are pushed away when the electrode is negatively biased, and almost no electrons exist near the electrode. This region is called the ion sheath, with the analogy being the sheath of a sword. In other words, an ion sheath refers to a sheath filled with ions. Because the electron density is very low in this reg... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The magnitude of voltage induced at the electrodes is dependent on the ratio of the electrode surface areas. Say that the surface areas of electrodes 1 and 2 are S1 and S2, respectively, and the voltages induced at each electrode are V1 and V2, respectively, as shown in Fig. 2.7. Their relationship [4] would be
$${\fr... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 2.2.2 Ion Scattering In The Sheath
Let's now quantitatively examine the scattering of ions in the sheath. The ion sheath thickness (dis) is represented by the following Child–Langmuir equation [5]:
$$d_{\mathrm{{in}}}={\frac{2}{3}}{\Bigg(}{\frac{\varepsilon_{0}}{i_{\mathrm{{lo}}}}}{\Bigg)}^{\frac{1}{2}}{\Bigg(}{\f... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Another important concept in examining the scattering of ions in the sheath is the mean free path (λ), which we briefly discuss here. A mean free path is an average distance that a particle travels from one collision to the next. In other words, it is the distance over which a particle is able to travel without a colli... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
In other words, λ is much larger compared to d d is is l = æè ç öø
÷ 0. , 056 and the majority of ions arrive at the surface of the sample without colliding with neutral particles in the sheath (Fig. 2.9a). On the other hand, λ is smaller than dis in the batch RIE
dis l = æè ç öø
÷ 3 8. , and most of the ions collide ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
ECR Plasma Etcher (0.4 Pa) **Fig. 2.11** Etch rates of contact holes as a function of hole diameter and operating pressure in three different etches [6]

in the etch rate is 40 % at a diameter of 0.4 μm. On the other hand, the ECR plasma etcher with a low operating pressure of 0.4 Pa ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Next, the CF3 radicals adsorb on the Si surface and react with Si to form etch byproducts SiF4. SiF4 desorbs from the Si surface, and the etching thus proceeds.
In order to realize fine patterning, it is important to process with a high level of fidelity to the mask patterns. Figure 2.13 illustrates the differences be... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

place, the etch rate of an ion-irradiated surface is significantly larger than the etch rate by neutral radicals. Therefore, an anisotropic etching is realized by making the ions strike the etch target surface at normal incidence.
Figure 2.14 shows the experimental result that explai... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Because the rate of etching through the ion-assisted reactions is orders of magnitude larger than the rate of etching by radicals, as thus shown, it is possible to obtain an anisotropic etch profile when ions come in on the wafer vertically, so that the etch rate in the vertical direction (by assisted reactions) is fas... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

Chemical etching driven by radicals is not dependent on the energy, and so the rate always remains constant. The etch rate is also low. The etch rate of ion-assisted etching is extremely dependent on the ion energy, and the etch rate drastically increases with increasing ion energy. A... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


etching of poly–Si gates and shallow trench isolations (STIs). On the other hand, etching tends to become isotropic when Si is etched with gases like SF6 and CF4, which dissociate and generate the F+ ions.
We'll now consider Al etching. According to... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Figure 2.18 shows a model illustrating the sidewall protection process [11]. In this example, the protective film consists of organic polymers. In the case of using a mixture gas in which a gas for polymer formation is added to a main etch gas, monomers such as CF and CF2 are generated from the additive gas. These mono... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
In reality, however, an anisotropic profile is obtained. The reason for this is a supply of C and H resulting from the resist being etched, which forms the sidewall protection film.
As mentioned earlier, the effect of ion-assisted reactions is very small when Si is etched using an F-based gas like SF6. In this case, S... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
easily and the etch rate becomes higher. Data in Table 2.3 show the melting and boiling points for various halides [12]. They also show that the fluorides of Si and W tend to vaporize more easily than the chlorides. However, there is an opposite trend with Al, and the fluorides are less easy to vaporize than the chlori... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
This is described in detail in the section on poly–Si etching in the next chapter. Furthermore, another effective approach might be to lower the ion energy in a gas system in which the etch rate dependence on the ion energy is strong for SiO2 and weak for poly–Si. An F-based gas is the case in point. | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| Chemical | compound Temperature (°C) | 85.2 | 223.5 | SiCl4 –34.7 SiClF3 –127.0 SiCl2F2 –102.9 SiCl3F –68.3 | SiF4 –130.4 | 72.7 | 10.0 | SnH4 –118.5 175.8 | 1,359 | | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| SbI3 | SnI4 | | | | | | | | | | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| HgI2 | KBr | KCl | LiBr | NaF | NaI | PbI2 | PbF2 | | | | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| CrO Cl 2 2 Cu Br 2 2 Cu Cl 2 2 | GeBr4 | HgBr2 HgCl2 | | | | | | | | | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| AgI | AlF3 AlI3 | CdF2 | | | | | | | | | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
2.3 How to Design Dry Etching Processes
## 2.3.6 Summary
As thus explained, when designing a dry etching process, the etching gas selection and reaction control should be chosen by considering the ion energy dependence of the chemical sputtering yield, the vapor pressures of the etch byproducts, and the atom-to-atom ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
10. S. Tachi and S. Okudaira: J. Vac. Sci. Technol. B 4, 459 (1986). 11. K. Nojiri, M. Sadaoka, H. Azuma, K. Kawamura: Ext. Abstr. 36th Spring Meeting of The Japan Society of Applied Physics, No. 2, p.571 (1989).
12. Rikagaku Jiten (Physics and Chemistry Dictionary) 3rd Edition, Iwanami Shoten (1981). 13. Y. Kawamoto:... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
12. Rikagaku Jiten (Physics and Chemistry Dictionary) 3rd Edition, Iwanami Shoten (1981). 13. Y. Kawamoto: Data Book on Submicron Lithography, Science Forum, p.335 (1985). 14. Kagaku Binran (Handbook of Chemistry): Maruzen Publishing Co., Ltd. 15. Handbook of Chemistry and Physics 47th Edition: The Chemical Rubber Co. ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The etching mechanism for SiO 2 material is different from that for the Si material, requiring a different plasma source. This chapter provides an in-depth review of the etching mechanism and the key parameters that dominate the etching process and offers insight into how to design the gas chemistry and the reasons why... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.1.1 Poly–Si Gate Etching
Conventionally, chlorofl uorocarbon or freon-based gases have been widely used for gate etching [ 1 ]. However, as we discuss later, etching with chlorofl uorocarbon makes it diffi cult to achieve a high selectivity to the gate oxide fi lm, because carbon in the gas promotes the etching ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
| Table 3.1 Bond strength for Si, SiO, halogenated Si, and CO [ 2 ] |
|-----------------------------------------------------------------------|
| C–O | (kcal/mol) | | |
|------------|--------------|-------|------|
| 257 a | Si–F | 132 a | |
| –Si–O– | 111 b | Si–Cl ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.1.2 Across-Wafer Critical Dimension Uniformity Control
The across-wafer CD uniformity is strongly affected by the redeposition of reaction byproducts onto the patterns [ 4 ]. Figure 3.2 illustrates how the redeposition of reaction byproducts on the patterns affects the CD. Two key parameters determine the CD uni... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


Fig. 3.3 Impact of the direction of gas injection on CD [ 5 ]
3 Dry Etching of Various Materials

while the patterns at the periphery are thicker. When the gas is injected toward the periphery of the wafer, the un... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.1.3 Wsi 2 /Poly–Si Gate Etching
A WSi 2 /poly–Si structure is referred to as a polycide gate and is widely used in DRAMs. A DRAM gate is a word line, and WSi 2 is used here to reduce the word line resistance. With the WSi 2 /poly–Si structure, it is necessary to etch vertically without any side etching into the ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


| RF Power | 80 W | 80 W |
|----------------|------------|------------------------|
| Etching Gas | Cl2 | Cl2+O2 (10%) 0.5 mm 50 |
| Etch Rate | 350 nm/min | 400 nm/min |
| Selectivity | ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
This result shows that the sidewall protection fi lm is SiO x . As indicated in Table 3.1 ,
since the bond strength of the Si–O bond is larger than that of the Si–Cl bond, Cl radicals barely etch the sidewall protection fi lm. Therefore, the sidewall protection fi lm effectively protects the sidewalls from the attacks... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

These results would lead to a theory that the reduction in the SiO 2 etch rate, due to the O 2 addition, is also caused by the SiO x deposition.
As discussed above, the O 2 addition is effective not only for increasing the WSi 2 etch rate and the poly–Si/SiO 2 selectivity, but also... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Fig. 3.9 High-temperature

etching of W/WN/poly–Si gate [ 9 ]. (W/WN was etched at 100 °C)
## 3.2 Silicon Dioxide Etching
There is a wide variety of applications in SiO 2 etching, including the etching of holes such as contact holes and via holes, hard mask etching for the STI an... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.2.1 Mechanism Of Silicon Dioxide Etching
For SiO 2 etching, C and F are necessary, and the etching gas is based on fl uorocarbon containing C and F. Furthermore, H 2 - or H-contained gas is added to the fl uorocarbon gas in order to obtain a large selectivity to the underlying Si. The reason for this mixture is ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Let's now look at the reactions taking place at the Si surface. Hydrogen radicals extract F from CF 3 adsorbed on the Si surface, and as a result, fl uorocarbon


polymers are formed. Because the Si surface is covered with polymer, the etching of Si ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Similar effects to those described here may also be achieved using gases such as CHF 3 , which itself contains H. Trifl uoromethane (CHF 3 ) is widely used as an SiO 2 etching gas. Furthermore, because the selectivity tends to increase in gases with a larger C ratio, as described in the next section, fl uorocarbons suc... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

ne : Electron density (Plasma density)
$$(3.1)$$
The number of collisions between the electrons and molecules can be expressed by the following equation:
$$\xi=\tau\cdot n_{\mathrm{e}}<\sigma\nu>,$$
xt s =× < > ne n , ( 3.1 )
where τ is the residence time of the particles, ne is ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The residence time of the particle τ is expressed with the following equation:
$$\tau={\frac{P V}{Q}},$$
$$(3.2)$$
t = PVQ , ( 3.2 )
where P is the pressure, V is the plasma volume, and Q is the gas fl ow rate.
In order to make τ smaller, the plasma volume should be small, the gas fl ow rate should be large, and ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The double-near-surface model [ 14 ] shown in Fig. 3.15 provides another explanation for the reason why a narrow-gap parallel-plate etcher is suitable for the SiO 2 etching. According to this model, the reactions taking place at the upper electrode


... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.2.3 Hole Etching
The next discussion covers the etching of holes, such as contact holes, via holes, and DRAM capacitor cells.
As Fig. 3.16 shows, gate contact holes are shallow and substrate contact holes are deep in a logic device, and the simultaneous etching of contact holes with varied depths is required.... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


Selectivity
the Si surface. This effect becomes more signifi cant with a lower Vmax . When Vmax is 200 V or less, the Si surface is completely covered with polymer, and Si etching stops; that is, the selectivity is infi nite. However, because the SiO... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


the following measures [ 18 ]. First, deposit thicker CF 2 polymer on the sidewall by increasing the CF 2 concentration in the plasma. The same approach described earlier should be utilized. Next, transport more C to the bottom by reducing the sticki... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

## 3.2.4 Self-Aligned Contact Etching
Self-aligned contact (SAC) etching is a technology for opening contact holes between the gate electrodes, as Fig. 3.21 shows. The gates are covered with an Si 3 N 4 fi lm, which functions as an etch stopper, so that the contact hole and the gate... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Octafl uorocyclopentene (C 5 F 8 ) has also gained attention as an alternative gas to C 4 F 8 . There has been a report of a selectivity of 21 at the Si 3 N 4 shoulder using a C 5 F 8 /O 2 gas chemistry in the magnetron RIE [ 21 ]. A high selectivity is believed to be achieved through the deposition of C-rich polymers ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

C3F5
Fig. 3.23 Relative concentration of chemical species in C 4 F 8 , C 4 F 8 /CO, and C 4 F 8 /H 2 plasma [ 20 ]

(1) Gate formation
(2) CVD dielectric deposition

(3) Spacer etching
, which blocks etching. In order to remove this oxi... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
A stacked metal layer structure of an Al alloy and a barrier metal is used for electromigration-resistance enhancement. Sometimes a thin fi lm is formed on top of the Al alloy as an antirefl ection fi lm. Specifi cally, the structure is a sandwich of, for example, TiN/Al–Si–Cu/TiN or TiW/Al–Si–Cu/TiW.
In Al etching,... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

polymers and increases the amount of side etching. This phenomenon, in which the side etching is caused by the decline in the supply of polymers from the resist, is observed on the actual device patterns in which the area of the resist mask is smaller compared to the area that is to ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Figure 3.27 shows the Vdc dependence of the Al–Si–Cu etch rate and the side etching amount in an ECR plasma [ 24 ]. The pressure is 1.3 Pa. The fi gure shows that it is possible to control the amount of side etching without changing the etch rate, by adjusting the Vdc . Figure 3.28 shows an example of a stacked metal l... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
Figure 3.29 shows the amount of residual Cl on the wafer as a function of process step of Al–Si–Cu etching [ 27 ]. More than 99 % of the residual Cl can be removed when the resist is stripped off by an asher. When this step is followed by a wet cleaning, the Cl concentration goes back to almost the pre-etching level. W... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 3.4 Summary
The discussions in this chapter have focused on gate etching, SiO 2 etching for holes, spacer etching, and etching of Al alloy stacked metal layer structures, which are the key technologies in the semiconductor manufacturing process. These discussions have delved into details on the key parameters for ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
6. K. Nojiri, C. Lee, V. Vahedi, R. A. Gottscho: Proc. SEMI Technol. Symp. p.6-14, (2004). 7. K. Nojiri, K. Tsunokuni and K. Yamazaki: J. Vac. Sci. Technol., B14, 1791 (1996). 8. T. P. Chow and A. J. Steckl: J. Electrochem. Soc. 131, 2325 (1984). 9. K. Nojiri, N. Mise, M. Yoshigai, Y. Nishimori, H. Kawakami, T. Umezawa... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
19. T. Tatsumi, M. Matsui, S. Kobayashi, L. Wang, S. Noda and M. Sekine: Proc. Symp. Dry Process, p.297 (1999).
20. T. Sakai, H. Hayashi, J. Abe, K. Horioka and H. Okano: Proc. Symp. Dry Process, p.193
(1993).
21. Y. Ito, A. Koshiishi, R. Shimizu, M. Hagiwara, K. Inazawa and E. Nishimura: Proc. Symp. Dry Process... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
## 4.1 History Of Dry Etching Equipment
The dry etching equipment fi rst used in semiconductor manufacturing as an alternative to wet etching was a barrel-type plasma etcher. In this system, plasma is generated with an electromagnetic induction coil or capacitively coupled electrodes placed around a cylindrical quart... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The fi rst method utilized for increasing the plasma density in single-wafer dry etching equipment was the magnetron RIE. This is a method of enhancing the plasma density with the application of a magnetic fi eld and is also referred to as MERIE, for magnetically enhanced reactive-ion etching. This method has little ma... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
An ECR plasma etcher requires a large magnetic coil to form a strong magnetic fi eld, which makes it diffi cult to make the etch chamber compact. The ICP etcher was developed to address this issue. A simple coil was placed on top of the etch chamber to generate a high-density plasma by electromagnetic induction. The IC... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The subsequent sections in this chapter include detailed discussions of the dry etching equipment used for LSI manufacturing.
## 4.2 Barrel-Type Plasma Etcher
Figures 4.1 and 4.2 show the cross-sectional diagrams for the barrel-type plasma etchers. This system has an electromagnetic induction coil (Fig. 4.1 ) or a ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


## 4.3 Capacitively Coupled Plasma Etcher
Figure 4.3 shows a cross-sectional diagram of a CCP etcher. Plasma is generated by applying RF power on a pair of electrodes that are placed in parallel with each other. This type of etcher is also referred... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||


## 4.4 Magnetron Reactive-Ion Etching
Magnetron RIE is a method of generating a high-density plasma through the cycloid motion of electrons resulting from mutual interactions between the electrical and the magnetic fi elds. The equipment structure ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||
The magnetron technology is capable of generating a high-density plasma even at a low pressure. However, it has some drawbacks. First, ion energy cannot be controlled independently of the plasma discharge, because the plasma discharge and the ion energy control are carried out with a single RF power supply. Second, it ... | text_only | 15_dry-etching-technology-for-semiconductors_compress | ||

## 4.5 Electron-Cyclotron Resonance Plasma Etcher
An ECR plasma etcher has advantageous features, such as high-density plasma generation at a low pressure and independent control of ion energy and plasma discharge. These features are suited for fi ne pattern etching. The production ... | text_only | 15_dry-etching-technology-for-semiconductors_compress |
Subsets and Splits
No community queries yet