![74_image_0.png](74_image_0.png) ![74_image_1.png](74_image_1.png) plasma discharge through an RF power applied to the wafer stage, and a closely controlled fi ne patterning is possible. Because the ECR plasma uses the magnetic fi eld, however, charging damage occurs under some conditions. This issue can be resolved...
text_only
15_dry-etching-technology-for-semiconductors_compress
Because the ICP etcher is able to provide a high-density plasma without a large electromagnetic coil as in an ECR plasma etcher, it has become the mainstream etching equipment for processing conductive materials such as gates, Si (e.g., STI), and Al lines. ![76_image_0.png](76_image_0.png) ![76_image_1.png](76_image...
text_only
15_dry-etching-technology-for-semiconductors_compress
![78_image_0.png](78_image_0.png) ## 4.8 Electrostatic Chuck Finally, we will discuss the electrostatic chuck, which plays an important role in dry etching equipment. The electrostatic chuck is sometimes referred to as the ESC. In etching equipment today, the electrostatic chuck is usually used as the lower electrod...
text_only
15_dry-etching-technology-for-semiconductors_compress
Fig. 4.13 Cross-sectional structures and clamping mechanisms for monopolar and bipolar electrostatic chucks 4 Dry Etching Equipment ![79_image_0.png](79_image_0.png) force between positive and negative charges. With the monopolar structure, the wafer receives electrical charges from the plasma for clamping. In other ...
text_only
15_dry-etching-technology-for-semiconductors_compress
![80_image_0.png](80_image_0.png) ![80_image_1.png](80_image_1.png) chucking and dechucking responses. However, the clamping force is small, and a high voltage is required for the clamping. The resistivity is not dependent on temperature. With the Johnsen–Rahbek electrostatic chuck, a material of some level of ele...
text_only
15_dry-etching-technology-for-semiconductors_compress
## 4.8.2 Principle Of Wafer Temperature Control The temperature of the wafer is controlled indirectly through a thermal contact between the temperature-controlled lower electrode (electrostatic chuck) and the wafer backside. Figure 4.16 shows the principle of wafer temperature control. The electrostatic chuck is main...
text_only
15_dry-etching-technology-for-semiconductors_compress
1. K. Nojiri: Electronic Journal 90th Technical Symposium, p.89 (2004). 2. M. Sekine, M. Narita, S. Shimonishi, I. Sakai, K. Tomioka, K. Horioka, Y. Yoshida and H. Okano: Proc. Symp. Dry Process, p.17 (1993). 3. K. Nojiri and K. Tsunokuni: J. Vac Sci. Technol., B 11, 1819 (1993). 4. S. Nakagawa, T. Sasaki, and M. Mo...
text_only
15_dry-etching-technology-for-semiconductors_compress
# Chapter 5 Dry Etching Damage Dry etching has been a key technology in the LSI manufacturing process, and the high integration of LSI would not have been realized without progress in this technology. However, because the process uses plasma, the devices are susceptible to various types of damages caused by high-ener...
text_only
15_dry-etching-technology-for-semiconductors_compress
During dry etching, impurities such as heavy metals are released into the plasma from the etch chamber or the electrode, either by sputtering or by chemical reactions. These impurities or molecules in the etching gas are injected into the Si substrate in the form of ions. In SiO 2 etching using fl uorocarbon-based gase...
text_only
15_dry-etching-technology-for-semiconductors_compress
remain within an approximately 10-nm range from the surface [ 1 ], but H penetrates deeper. It has been reported that H was present at a depth of 50 nm with a reactiveion etching (RIE) using CF 4 + H 2 gas chemistry [ 2 ]. Figure 5.2 shows the result of a high-resolution transmission electron microscope analysis on the...
text_only
15_dry-etching-technology-for-semiconductors_compress
![84_image_0.png](84_image_0.png) Fig. 5.2 High-resolution ![85_image_0.png](85_image_0.png) transmission electron microscope photograph of the Si surface layer damaged in a narrow-gap parallel-plate plasma etcher. *Arrows* indicate crystalline defects [ 3 ] ![85_image_1.png](85_image_1.png) ![86_image_0.png](8...
text_only
15_dry-etching-technology-for-semiconductors_compress
## 5.2 Charging Damage Gate oxide breakdown caused by wafer charging is becoming a serious problem as the gate oxides become thinner. Figure 5.6 shows the frequency of gate oxide breakdown as a function of the gate oxide thickness when a negative wafer charging occurs in a barrel asher [ 8 ]. The parameter ΔVFB is a ...
text_only
15_dry-etching-technology-for-semiconductors_compress
![87_image_0.png](87_image_0.png) ## 5.2.1 Evaluation Method Of Charging Damage The wafer charging resulting from a plasma treatment can be monitored using MNOS capacitors [ 9 ]. Figure 5.7a shows the structure of an MNOS capacitor [ 10 ]. When this MNOS capacitor is exposed to a plasma, the gate electrode is charge...
text_only
15_dry-etching-technology-for-semiconductors_compress
## 5.2.2 Mechanism Of Wafer Charging When the distribution of the RF current fl owing onto the wafer surface is nonuniform across the wafer, wafer charging occurs [ 10 ]. For example, when the RF current fl owing onto the wafer is higher at the wafer peripheral than at the center, ![88_image_0.png](88_image_0.png...
text_only
15_dry-etching-technology-for-semiconductors_compress
![90_image_0.png](90_image_0.png) ![90_image_1.png](90_image_1.png) distribution of RF current. They may include a nonuniformity in the plasma density, orientations of the electrical fi eld and magnetic fi eld with respect to the wafer, and their distributions. In the case of the magnetic fi eld, the current tends to...
text_only
15_dry-etching-technology-for-semiconductors_compress
![91_image_0.png](91_image_0.png) ![91_image_1.png](91_image_1.png) capacitors show the intrinsic breakdown voltage. In other words, the gate oxide breakdown did not occur during plasma treatment. On the other hand, when the magnetic fi eld is applied, a positive charging, corresponding to ΔVFB = +4.5 V, occurs exce...
text_only
15_dry-etching-technology-for-semiconductors_compress
## Ecr Plasma Etcher In an ECR plasma etcher, simply generating a uniform plasma is insuffi cient to prevent the wafer charging. Figure 5.16 shows the cross-sectional diagram of an ECR plasma etcher, and Fig. 5.17 shows the across-the-wafer distribution of ΔVFB after plasma treatment in this etcher [ 10 ]. When no RF...
text_only
15_dry-etching-technology-for-semiconductors_compress
![95_image_0.png](95_image_0.png) ![95_image_1.png](95_image_1.png) Fig. 5.20 Schematic diagram of TCP® plasma etching apparatus [ 13 ] 200-mm wafers etched at 800 kHz and 2 MHz [ 3 ]. At 2 MHz, the gate oxide breakdown occurs at the center of the wafer, and the area surrounding the center shows the degradation of ...
text_only
15_dry-etching-technology-for-semiconductors_compress
As discussed so far, the wafer charging can be prevented by making the distribution of the RF current fl owing on the wafer surface uniform. By doing so, it is possible to eliminate the wafer charging even for a high-density plasma using a strong magnetic fi eld as in the ECR etcher. ## 5.2.4 Pattern-Dependent Gate O...
text_only
15_dry-etching-technology-for-semiconductors_compress
An effective way to reduce the electron shading damage is to reduce the electron temperature. This can be done by widening the gap between the electrodes and/or ![97_image_0.png](97_image_0.png) ![98_image_0.png](98_image_0.png) raising the pressure [ 16 ]. More effective methods to reduce the electron shading dama...
text_only
15_dry-etching-technology-for-semiconductors_compress
The most serious charging damage occurs during the etching and ashing steps for the metal lines of logic LSI, because long metal lines that could act as antennae are connected to the gates. As discussed in Fig. 5.9 , the breakdown frequency increases with an increased antenna ratio. To address this, some of the measure...
text_only
15_dry-etching-technology-for-semiconductors_compress
6. K. Hashimi, D. Matsunaga, M. Kanazawa: Ext. Abstr. 54th Fall Meeting of The Japan Society of Applied Physics, No. 2, p.536 (1993). 7. N. Aoto, M. Nakamori, H. Hada, T. Kunio, and E. Ikawa: Ext. Abstr. Int. Conf. Solid State Devices and Materials, p.101 (1993). 8. K. Tsunokuni, K. Nojiri, S. Kuboshima and K. Hi...
text_only
15_dry-etching-technology-for-semiconductors_compress
19. K. Noguchi: Electronic Journal 8th Technical Symposium, p.31 (1997). 20. M. Takebuchi, K. Yamada, T. Nishimura, K. Isobe, T. Uemura, T. Fujimoto, M. Arakawa, S. Mori, A. Kimitsuka and K. Yoshida: Tech. Dig. Int. Electron Devices Meet., p.185 (1996). # Chapter 6 Latest Dry Etching Technologies This chapter revie...
text_only
15_dry-etching-technology-for-semiconductors_compress
## 6.1 Copper Damascene Etching The speed of logic LSI devices has been increased mainly via scaling of transistors. However, metal lines became the limiting factor on the speed of LSI devices starting at the 0.25-μm node [ 1 ]. Figure 6.1 shows the reason for this. With more scaling (and higher levels of integrat...
text_only
15_dry-etching-technology-for-semiconductors_compress
A new technology called damascene was introduced for forming the Cu metal lines. Cu introduction Line resistance R1< R2 Countermeasure Low-k film introduction ![101_image_0.png](101_image_0.png) 1. The fi rst-layer Al metal lines have been formed. 2. An interlayer insulating fi lm is deposited and planarized by...
text_only
15_dry-etching-technology-for-semiconductors_compress
![102_image_0.png](102_image_0.png) schemes of dual-damascene, and Fig. 6.3 shows the via-fi rst scheme that has become the mainstream technology these days, whose steps follow: 1. The fi rst-layer Cu metal lines have been formed. 2. A barrier fi lm (SiN), for preventing the diffusion of Cu, is deposited on top of Cu,...
text_only
15_dry-etching-technology-for-semiconductors_compress
dielectric constant goes up, and the benefi t of using a low-κ fi lm is reduced. For this reason, the stopper layer for etching is not used in most cases these days. In that case, it is necessary to achieve a stable etch rate, because the trench depth is determined by the etching depth. Figure 6.4 shows an example of t...
text_only
15_dry-etching-technology-for-semiconductors_compress
Fluorine-doped SiO 2 can be etched with almost the identical etching conditions as SiO 2 . The low-κ fi lm, with κ = 3.0 or less, was introduced in earnest at the 90-nm technology. A process combination involving low-κ fi lm makes the overall process technology more challenging, because the etching of low-κ fi lm itsel...
text_only
15_dry-etching-technology-for-semiconductors_compress
Here a methylsiloxan-based organic SOG is etched with a C 4 F 8 /O 2 /Ar gas chemistry. Figure 6.7 illustrates the mechanism of how the subtrenches are created [ 2 ]. As Fig. 6.7 (1) shows, the thickness of CF polymers deposited inside the trench is not uniform. It is thinner at the bottom corners of the trench. As a...
text_only
15_dry-etching-technology-for-semiconductors_compress
Figure 6.9 shows an example of dual-damascene etching on the same organic SOG using the optimized concentration of O 2 and C 4 F 8 [ 3 ]. The low-κ fi lm containing CH 3 requires special attention with ashing as well. As Fig. 6.10a shows, the oxygen radicals extract the CH 3 during ashing with an oxygen plasma [ ...
text_only
15_dry-etching-technology-for-semiconductors_compress
![107_image_0.png](107_image_0.png) ![107_image_1.png](107_image_1.png) ![107_image_2.png](107_image_2.png) organic polymer fi lms. There has been a report on the process in which the hard mask is opened using a resist mask, and then the resist is etched off during the etching of organic fi lm by O 2 reactive-ion et...
text_only
15_dry-etching-technology-for-semiconductors_compress
3. Then the resist is stripped off with an asher. Because the resist is stripped off at this step, there is no step for removing the resist after trench etching, and damage, therefore, is prevented. 4. Next, the resist patterns for the via holes are formed. 5. "BARC" in the fi gure refers to the bottom antirefl ecti...
text_only
15_dry-etching-technology-for-semiconductors_compress
![109_image_4.png](109_image_4.png) ![109_image_5.png](109_image_5.png) ![109_image_6.png](109_image_6.png) (8) Barrier etching BARC ![109_image_7.png](109_image_7.png) The reason to use a metal hard mask like TiN for trench etching in this process is to achieve a large selectivity to the porous low-κ fi lm. This...
text_only
15_dry-etching-technology-for-semiconductors_compress
There was also a problem with the gate electrode material. A depletion layer is formed in the conventional poly–Si gate and increases the effective gate insulating fi lm thickness. For this reason, metal gates, in which no depletion layer is formed, were introduced at the 45-nm node. Various materials were also investi...
text_only
15_dry-etching-technology-for-semiconductors_compress
With the gate-last method, a poly–Si gate is fi rst formed. After the heat treatment steps such as ion implantation, activation annealing, and silicidation are completed, the poly–Si gate is removed. The high-κ fi lm and metal are deposited into ![111_image_0.png](111_image_0.png) ![111_image_1.png](111_image_1.png)...
text_only
15_dry-etching-technology-for-semiconductors_compress
This section focuses on the etching technology for the gate-fi rst scheme, which has many challenges. Figure 6.14 shows the typical structure and materials that are used for the metal gate/high-κ [ 10 ]. The high-κ fi lms used are hafnium oxides, including HfO 2 , HfSiO 2 , and HfSiON. The metal used is TiN or TaN, and...
text_only
15_dry-etching-technology-for-semiconductors_compress
![113_image_1.png](113_image_1.png) Another issue that needs to be addressed is the La residues. As mentioned earlier, the LaO cap on the high-κ fi lm is used for the n-type MOS transistors. Because La etch byproducts are nonvolatile, they tend to lead to residues. These residues can usually be removed with wet clean...
text_only
15_dry-etching-technology-for-semiconductors_compress
Figure 6.19 shows a process fl ow for metal gate/high-κ etching for FinFETs [ 15 ]: 1. This is the cross section before poly–Si etching. 2. For the main etching, a highly anisotropic process is used for etching an 80-nmthick poly–Si fi lm by approximately 60 nm, but the etching is stopped before TiN is exposed. Th...
text_only
15_dry-etching-technology-for-semiconductors_compress
![115_image_0.png](115_image_0.png) ![116_image_0.png](116_image_0.png) Fig. 6.20 Etching profi le of metal gate/high-κ for FinFET [ 15 ] ![116_image_1.png](116_image_1.png) ## 6.6 Double Patterning The resolution in lithography technology is proportional to the wavelength of the light source. In other words, a...
text_only
15_dry-etching-technology-for-semiconductors_compress
![117_image_0.png](117_image_0.png) 1. First, the stacked fi lms, core fi lm, and hard mask are deposited on the Si substrate, and resist patterns are then formed using ArF immersion lithography technology. 2. Next, the hard mask is etched, and this hard mask is then used as a mask for etching the core fi lm. 3...
text_only
15_dry-etching-technology-for-semiconductors_compress
7. The stacked fi lm is etched using the sidewall spacers as a mask, and then the Si substrate is etched for completing the STI formation. 8. As thus shown, the sidewall transfer DPT makes it possible to create fi ne geometry patterns that are one half the pitch achieved at the lithography resolution limit. The p...
text_only
15_dry-etching-technology-for-semiconductors_compress
![119_image_0.png](119_image_0.png) Fig. 6.23 Three-dimensional Chip integrated circuit (3D IC) by chip stacking patterning requires a large number of process steps and the manufacturing cost increases. Also, even with double patterning, the lithography technology will hit another limit in resolution with further de...
text_only
15_dry-etching-technology-for-semiconductors_compress
Through-Si vias (TSVs) are used for chip-to-chip connections in the 3D IC. The TSV is deep, of approximately 50–100 μm, and the etching technology used for forming the TSV is called deep-Si etching. An etching method called the Bosch process is generally used for TSV etching. The Bosch process consists of a repetitio...
text_only
15_dry-etching-technology-for-semiconductors_compress
There is almost no visible scalloping. ![121_image_0.png](121_image_0.png) Fig. 6.26 Scanning electron microscope cross-sectional profi le of TSV formed by Bosch process [ 19 ] 1. M. T. Bohr: Tech. Dig. Int. Electron Devices Meet., p.241 (1995). 2. S. Uno, T. Yunogami, K. Tago, A. Maekawa, S. Machida, T. Tokunag...
text_only
15_dry-etching-technology-for-semiconductors_compress
16. K. Yahashi, M. Ishikawa, H. Oguma, M. Omura, S. Takahashi, M. Iwase, H Hayashi, I. Sakai, M. Hasegawa and T. Ohiwa: Proc. Symp. Dry Process, p.279 (2008). 17. R. Dejule: Semiconductor International, p.14, May (2009). 18. P. Marchal and M. V. Bavel: Semiconductor International, p.24, August (2009). 19. C. Rusu: 5...
text_only
15_dry-etching-technology-for-semiconductors_compress
As of 2014, devices with 20-nm-level minimum feature sizes had gone into volume production. This means that minimum feature sizes were scaled to 1/250 in 39 years. At the same time, the number of transistors on each microprocessor chip grew by approximately 100,000-fold. Furthermore, the Si wafer diameter, which used t...
text_only
15_dry-etching-technology-for-semiconductors_compress
The plasma used for dry etching causes charging damage, and at one time there was a concern that this problem could preclude the use of plasma for further scaling. Nevertheless, a great deal of active research work, mainly in Japan, took place in the late 1980s through the fi rst half of the 1990s on understanding the ...
text_only
15_dry-etching-technology-for-semiconductors_compress
The history of semiconductors includes a large number of technological innovations, not just in fi ne geometry processing, and the industry has commercialized many technologies that used to seem out of reach. As a result, it has achieved the prosperity seen today. There will be many more new technologies coming their w...
text_only
15_dry-etching-technology-for-semiconductors_compress
New types of memories are explored as an alternative to DRAM and fl ash memory, which suffer from a reduced number of stored charges as a result of scaling. Some of the new memory technologies being considered are phase change random access memory (PRAM), magnetoresistive random access memory (MRAM), and resistive ra...
text_only
15_dry-etching-technology-for-semiconductors_compress
Therefore, the gate etching technology of the future will require atomic-level control such as an atomic layer etching, in which one atomic layer is etched at a time. It will be impossible to meet these contradicting demands using a single etching method. Different types of etching equipment optimized for each type o...
text_only
15_dry-etching-technology-for-semiconductors_compress
2. K. Suzuki, Y. Kawasaki, Y. Kakehi, K. Nojiri, S. Shimizu: Report of 36th Okouchi Memorial Prize (1990). 3. K. Nojiri: Charging Damage in Semiconductor Process, p.51 (REALIZE INC, 1996). 4. H. Tanaka et al: Tech. Dig. Symp. VLSI Technology, p.14 (2007). 5. K. Eriguchi, A. Matsuda, Y. Nakakubo. M. Kamei, H. Ohta, K...
text_only
15_dry-etching-technology-for-semiconductors_compress
Engineers engaged in etching technology development must also know about the peripheral technologies, or other process technologies. They also need to deepen their understanding of device structures and device characteristics. For example, knowledge in both plasma and devices is required in order to understand plasma d...
text_only
15_dry-etching-technology-for-semiconductors_compress
HANDBOOK OF SILICON WAFER CLEANING LECHNOLOGY THIRD EDITION EDITED BY KAREN REINHARD T WERNER KERN Handbook of Silicon Wafer Cleaning Technology This page intentionally left blank # Handbook Of Silicon Wafer Cleaning Technology Third Edition Edited by Karen A. Reinhardt Cameo Consulting, San Jose, CA, USA Werner Kern...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Practitioners and researchers must always rely on their own experience and knowledge in evaluating and using any information, methods, compounds, or experiments described herein. In using such information or methods they should be mindful of their own safety and the safety of others, including parties for whom they hav...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## Section I Introduction And Overview 1. Overview and Evolution of Silicon Wafer Cleaning Technology Werner Kern 1.1 Introduction 4 1.2 Importance of Clean and Conditioned Wafer Surfaces 5 1.3 Overview of Wafer Contamination Aspects 10 1.4 Overview of Wafer Cleaning and Surface Conditioning Technology 14 1.5 Evol...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2.1 | Wafer Contamination | 88 | |------------|--------------------------------------|------| | 2.2 | Behavior and Impact of Contamination | 101 | | 2.3 | Sources of Defects and Contamination | 126 | | 2.4 | Summary | 141 | | References | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
# Section Iii Dry Cleaning Processes 6. Gas-Phase Wafer Cleaning Technology Antonio L.P. Rotondaro, Anthony J. Muscat 6.1 Introduction and Overview 306 6.2 Chemistry and Mechanisms 313 6.3 Removal of Silicon Oxides With HF Vapor 316 6.4 O3 and UV/O3 for Organic Removal, Resist Stripping, and Surface Oxidation 336 6.5 ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 10. Metal Surface Chemical Composition And Morphology Jin-Goo Park, Nagarjuna R. Paluvai, R. Prasanna Venkatesh 10.1 Introduction 579 10.2 Aluminum 581 10.3 Copper 590 10.4 Tungsten 600 10.5 Cobalt 606 10.6 Summary 610 References 610 ## 11. Monitoring Of Chemicals And Water Joel L. Bigman, Karen A. Reinhardt 11.1...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
# List Of Contributors Kaveh Bakhtari, Transient Electronics Inc., Brookline, MA, United States Twan Bearda, IMEC, Leuven, Belgium Stephen P. Beaudoin, Purdue University, West Lafayette, IN, United States Joel L. Bigman, CI Semi, Migdal HaEmek, Israel Brian Brown, Applied Materials, Inc., Santa Clara, CA, United State...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
# Foreword* Cleaning of surfaces in semiconductor device processing has been of critical importance since the late 1950s and early 1960s. The reduction of stability, reliability, and device or circuit yield because of impurities incorporated during processing established that effective and efficient cleans were impera...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The criticality of cleaning increased as feature sizes decreased and as aspect ratios and the number of process steps for state-of-the-art devices increased. In addition, recognition that physical and chemical properties of surfaces played a crucial role in controlling subsequent film deposition and interface propertie...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Lower concentrations of reactive chemicals are typically used, while energy in the form of ion bombardment, mechanical agitation, and liquid or particle jets is supplied to the surface to assist residue removal. Because of the thin films and exposed interfaces in current devices, even these assisted processes can ## X...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Frequently, these sequences employ combinations of vapor or plasma steps along with liquid techniques. When the first edition of this Handbook was published in 1993, the intent was to collect information on semiconductor wafer cleaning and allied subjects from a variety of sources and make this information available i...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In this third edition, extensive updates and new approaches are included that reflect the current limitations and requirements of cleaning novel devices and materials (e.g., FinFETs, 3D devices, Co, III-V compounds), photoresist and residue removal, surface conditioning, and post-CMP cleaning. We expect that the covera...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Dennis W. Hess School of Chemical and Biomolecular Engineering Georgia Institute of Technology Atlanta, GA USA This page intentionally left blank # Preface And Acknowledgments* The first edition of this well-received handbook was published in 1993, edited by Werner Kern, the inventor of the RCA critical cleaning proc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
This handbook is meant as a guide for the personnel involved in integrated circuit manufacturing. The content of the handbook targets the engineers, technicians, and managers who work with cleaning and surface conditioning processes on a daily basis; developers who work on new technologies and manufacture products; and...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
I profusely thank the authors for taking their valuable time, some of which is beyond what their employers compensate, to research and then write the updated chapters. The new authors are also specially thanked for volunteering to outline, research, and write the new chapters, a daunting task that takes significant tim...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Chapter Outline 1.1 Introduction | 4 | | | | | |------------------------------------|------------------------------------------------------------------------------|----|-------|--------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 1.3.4 | Prevention of Contamination and Defectivity | 13 | | | | | 1.4 | Overview of Wafer Cleaning and Surface Conditioning Technology | 14 | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 1.4.3.1 | Ohmi Clean | 21 | | | | | 1.4.3.2 | IMEC Clean | 22 | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
* Revised by Karen A. Reinhardt Handbook of Silicon Wafer Cleaning Technology. https://doi.org/10.1016/B978-0-323-51084-4.00001-0 Copyright © 2018 Elsevier Inc. All rights reserved. 3
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 1.4.5 | Wafer Rinsing, Drying, and Storing | 27 | | | | |------------|-----------------------------------------------------------------|------|---------|--------------------------|----| | 1.4.5.1 | Wafer Rinsing ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 1.5.2.1 | Radiochemical Studies of Surface Contamination | 38 | | | | | 1.5.3 | Period from 1972 to 1989 | 47 | | | | | 1.5.3.1 | Chronological Survey of the Literature on H2O...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 1.1 Introduction The preparation of ultraclean Si (silicon) surfaces by cleaning and surface conditioning for the manufacturing of integrated circuits (ICs) has undergone considerable changes since we published the first edition of this handbook in 1993. The driving forces for these changes have been the ever-incre...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The understanding of surface contamination and defectivity and the role of particle adhesion, deposition, measurement, and removal have been substantially advanced during the past 14 years. The same is true for the ancillary analytical and control aspects, including the elucidation of the chemical composition of Si and...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 1.2 Importance Of Clean And Conditioned Wafer Surfaces The importance of clean substrate surfaces in the fabrication of semiconductor microelectronic devices has been recognized since the dawn of solid-state device technology in the 1950s. It is now well known that the device performance, reliability, and product y...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The term "ultraclean" may be defined in terms of the concentration of both chemical contaminants and particles on the wafer surface. The International Technology Roadmap for Semiconductors (ITRS) [1,2] specifies metrics that define the impact on yield based on contamination and defectivity for both front end of line (F...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The term "surface conditioning" may need some clarification. In recent years, one has become to realize that the process of cleaning may do more than just remove impurities from the surface. It can prepare the surface chemically for the next process step. For example, immersing a Si wafer with a contaminated native (am...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In addition, cleaning technologies that are solvent-based, such as postetch cleaning where metal patterns are exposed and post-CMP (chemical mechanical polishing) cleaning, are evolving to use semiaqueous solvent chemistries that are more amenable to these requirements. The development of wafer cleaning technology had...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Others include the International Symposia on Ultra-Clean Processing of Silicon Surfaces; The Fine Particle Society; Sematech Surface Preparation and Cleaning Conference, Semiconductor Equipment and Materials International; MICRO, formerly Microcontamination; Semiconductor Pure Water and Chemicals Conference; the Instit...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 1.2.2 Wafer Cleaning And Surface Conditioning For Integrated Circuit Manufacturing The manufacturing of an IC requires 500e800 process steps, depending on the specific type of device. Most steps are performed as unit processes with the complete wafers before dicing them into individual chips. Approximately 15%e20% ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
"MOL" refers to "middle of line" and also to MEOL (mid end of line) and is the formation of metal-based gate structures and self-aligned contacts and metal 1 layer that connects these structures. Cleaning of these structures requires penetrating higheaspect ratio structures to clean the bottom of the contacts, for exam...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
A general basic cleaning process flow for ULSI production can be outlined as follows with detailed chemistry formulations to be discussed in Section 1.4.2: 1. Front End of Line (FEOL) a. Plasma-stripping photolithographic mask and impurities after ion implantation or etching b. Aqueous-based residue removal and cleanin...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
a. Plasma-stripping photoresist mask and impurities after pattern etching b. Poststripping cleaning using organic solvents or aqueous/organic solvent mixtures (semiaqueous solvents), in most case after plasma stripping c. Predeposition cleaning with brush scrubber, megasonic treatment in DIW application of cryogenic ae...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
A specialized cleaning operation is required for Si device wafers after CMP. Depending on the metallization used for the device, the exposed surface may consist of Al, Cu, or W in addition to Si, SiO2, silicate glasses and doped glasses, SiNx, Si3N4, diffusion barrier layers such as TaN and TiN, etch stop films, and p...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 1.3 Overview Of Wafer Contamination Aspects The contamination of Si wafer surfaces is intimately associated with wafer cleaning and surface conditioning because this is the very reason for cleaning. Chapter 2 discusses this subject in depth, covering both chemical and particle contamination and the resulting defec...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Particles can originate from airborne dust from equipment, processing chemicals, factory operators, gas piping, wafer handling, and film deposition systems. Mechanical (moving) equipment and containers for liquids are especially prolific sources, whereas solid materials, liquids, gases, chemicals, and ambient air tend ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In this connection, we should mention that a small fraction of wafers in the fabrication of solid-state microelectronic devices utilize compound semiconductors such as gallium arsenide (GaAs), gallium phosphide (GaP), and numerous complex alloys. The importance of these materials has grown steadily for unique applicati...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Molecular contaminant films on wafer surfaces can act as a mask and thereby prevent effective cleaning or rinsing, impair good adhesion of deposited films, and on heating form deleterious decomposition products. For example, organic residues, if exposed to high temperatures in a nonoxidizing atmosphere, can carbonize a...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Impurity Elements From Chemicals and Processes in the Manufacturing of Si ICs Have Deleterious Effects on Device Performance Heavy metals (most critical) Cu, Fe, Ni, Cr, Co, Mo Alkali metals (critical) Na, K, Li, Ca Other elements (least critical) Al, Mg, C, S, CI, F | |---------------------------------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In advanced stages of device fabrication, particles can cause shorts between conductor lines if they are sufficiently large, conductive, and located between conductor lines. They are considered potential device killers if their size is larger than one-tenth the size of the smallest feature of the affected IC. ## 1.3.4...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Processing equipment has been the major source of particle contamination [62] and must be controlled effectively by eliminating the dust through scheduled maintenance and by electrostatic charge removal [20,62]. Particle generation can be further minimized by reducing friction of moving equipment parts, avoiding turbul...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Refined methods for the analysis of trace impurities on Si surfaces are available [75e84] to monitor the results of cleaning processes, as discussed in Chapter 10. ## 1.4 Overview Of Wafer Cleaning And Surface Conditioning Technology The topics discussed in this section include liquid processes, gas-phase methods, an...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Several comprehensive reviews have been published that cover this topic thoroughly [85e88]. Liquid methods of wafer cleaning are based on the application of mineral acids, aqueous solutions including H2O2-containing mixtures, organic solvents, and aqueous/solvent combinations. Different process sequences are used for ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 1.4.2 Wet-Chemical Cleaning Processes 1.4.2.1 Hydrofluoric Acid Solutions Mixtures of concentrated hydrofluoric acid (49 wt% HF) and DIW have been widely used for etching films of silicon dioxide (SiO2), silicate glasses (e.g., phosphosilicates, borophosphosilicates), and silicon nitride (Si3N4, SiNx) that were gro...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Mixtures of HF and ammonium fluoride (NH4F) solutions are known as buffered oxide etch (BOE or BHF) and are used for pattern delineation etching of oxide and glass films. Buffering results in a more stable etch rate and prevents loss of photoresist polymer films that cannot withstand strongly acidic unbuffered HF solut...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
These SPM, which are also known as "piranha etch" (because of their voracious ability to eradicate organics) or, incorrectly, "Caros acid," are extremely dangerous to handle in the fab; goggles, face shields, and plastic gloves are needed to protect the operators. This procedure is usually the first cleaning process to...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The first successful process for wet-cleaning FEOL Si wafers was systematically developed at RCA, used for several years in the fabs, and finally published in 1970 [101]. The process consists of two consecutively applied hot solutions known as "RCA Standard Clean," SC-1 and SC-2, featuring pure and volatile reagents. T...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The originally specified composition for the SC-1 solution ranges from 5:1:1 to 7:2:1 parts by volume of H2O:H2O2:NH4OH. Filtered DIW or quartzdistilled H2O is used. The H2O2 is electronic grade 30 wt% H2O2, unstabilized (to exclude contaminating stabilizers). The NH4OH is 27% (wt/wt% based on NH3). The originally spec...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The SC-1 solution was designed to remove from Si, oxide and quartz surfaces organic contaminants that are attacked by both the solvating action of the NH4OH and the powerful oxidizing action of the alkaline H2O2. The NH4OH also serves to remove by complexing some periodic group IB and IIB metals such as Cu, Au, Ag, Zn,...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress