[181] J.J. Rosato, R.N. Walters, R.M. Hall, P.G. Lindquist, R.G. Spearow, C.R. Helms, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 94e97 Third International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 94-7, The Electrochemical Society, Penningt...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[186] J.A. Fahremkrug, J.J. Rosato, C.R. Olson, P.G. Lindquist, in: Proceedings 6th International Symposium, SCP Global Technologies, Boise, Idaho, May 1999. [187] C.K. Chang, V. Nguyen, Q. Zhang, T.H. Foo, in: J. Ruzyllo, T. Hattori, R.L. Opila, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[196] M.B. Olesen, in: Proc. Institute of the Institute of Environmental Sciences, Ann. Tech. Mtg, 1990, p. 229. Mount Prospect, IL. [197] K. Anabuki, Y. Yamashita, T. Nawata, ECS Ext. Abstr. 90-2 (1990) 443. The Electrochemical Society, Pennington, NJ. [198] J. Marra, in: Extended Abstracts, 3rd Symposium on Partic...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[205] Y. Ma, M.L. Green, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 95e20 Fourth International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 95-20, The Electrochemical Society, Pennington, NJ, 1996, p. 115. [206] S. O'Brian, B. Bohannon, M.H. ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[210] J.M. De Larios, J.O. Borland, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 94e97 Third International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 94-7, The Electrochemical Society, Pennington, NJ, 1994, p. 347. [211] D.K. Hwang, J. Ruzyll...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[214] M.A. Lester, Semicond. Int. 23 (14) (December 2000) 46. [215] B.D. Schwab, R.W. Gifford, J.W. Butterbaugh, in: J. Ruzyllo, T. Hattori, R.L. Opila, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 2001-26 Seventh International Symposium on Cleaning Technology in Semiconductor Device Manufac...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[221] D.M. Mattox, Precis. Clean. (June 1996) 11. [222] P. Singer, Semicond. Int. 19 (8) (August 1996) 83. [223] C. Boitnott, Solid State Technol. 37 (10) (October 1994) 51. [224] R.E. Walkup, K.L. Saenger, G.S. Selwyn, J. Chem. Phys. 84 (1986) 2668. [225] S. Fujimura, M.T. Suzuki, K. Shinagawa, M. Nakamura, J. Vac....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[235] J.W. Butterbaugh, MICRO 20 (2) (February 2002) 23. See also: B.K. Kirkpatrick, E.C. Williams, S. Lavangkul, J.W. Butterbaugh, Electrochemical Society (ECS) Symposium Proceedings: 2001-26 Seventh International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, in: J. Ruzyllo, T. Hattori, R.L....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
First International Surface Cleaning Workshop, Northeastern University, Boston, MA, November 2002. [248] D.E. Koontz, C.O. Thomas, W.H. Craft, I. Amron, in: Symposium on Cleaning of Electronic Device Components and Materials, vol. 246, ASTM STP, 1959, p. 136. [249] D.O. Feder, D.E. Koontz, in: Symposium on Cleaning o...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[264] B.F. Philips, D.C. Burkman, W.R. Schmidt, C.A. Peterson, J. Vac. Sci. Technol. A1 (2) (1983) 646. [265] A.M. Goodman, L.A. Goodman, H.F. Gossenberger, RCA Rev. 44 (2) (1983) 326. [266] M. Watanabe, M. Harazono, Y. Hiratsuka, T. Edamura, ECS Ext. Abstr. 83e1 (1983) 221. The Electrochemical Society, Pennington, ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[275] I. Lampert, ECS Ext. Abstr. 87-1 (1987) 381. The Electrochemical Society, Pennington, NJ. [276] G. Gould, E.A. Irene, J. Electrochem. Soc. 174 (4) (1987) 1031. [277] J. Ruzyllo, J. Electrochem, Soc. 174 (4) (1987) 1869. [278] V. Probst, H.J. Bohm, H. Schaber, H. Oppolzer, I. Weitzel, J. Electrochem. Soc. 135 (3)...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[289] G. Duranko, D. Syverson, L. Zazzera, J. Ruzyllo, D. Frystak, in: B.E. Deal, C.R. Helms (Eds.), Physics and Chemistry of SiO, and Si-SiO, Interfaces, Plenum Publishing Corp., New York, NY, 1988, pp. 429e436. [290] G.G. Fountain, S.V. Hattangandy, R.A. Rudder, J.B. Posthill, R.J. Markunas, MRS Symp. Proc. 146 (19...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[300] M. Heynes, C. Hasenack, R. De Keersinaecker, R. Falster, Microelectron. Eng. 10 (1991) 235 see also M.M. Heyns, Microcontamination, 9 (4) (1991) 29. [301] M. Sakurai, J. Ryuta, E. Morita, K. Tanaka, T. Yoshimi, Y. Shimanuki, ECS Ext. Abstr. 901 (1990) 710. The Electrochemical Society, Pennington, NJ. [302] G.W....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[310] W.A. Syverson, M.J. Fleming, P.J. Schubring, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 90e99. First International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 90-9, The Electrochemical Society, Pennington, NJ, 1990, p. 10. [311] J.K. T...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[317] T. Ohmi, N. Miki, H. Kikuyama, I. Kawanabe, M. Miyashita, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 90e99. First International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 90-9, The Electrochemical Society, Pennington, NJ, 1990, p. 95....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[325] R. Reif, in: Proc. on Chemical Surface Preparation, Passivation, and Cleaning, Growth and Processing, Symp. B, Paper 7.1, Spring Mtg. of MRS, San Francisco, CA, April 12e16, 1992. [326] M. Lier, in: Proc. on Chemical Surface Preparation, Passivation, and Cleaning, Growth and Processing, Symp. B, Paper 1.1, Sprin...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[330] D. Frystak, J. Ruzyllo, in: J. Ruzyllo, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 92e12 Second International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 92-12, The Electrochemical Society, Pennington, NJ, 1992, p. 58. [331] E.Y. Chang, in: Proc. On C...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[336] T. Ito, R. Sugino, Y. Sato, M. Okuno, A. Osawa, T. Aoyama, T. Yamazaki, Y. Arimoto, in: Proc. On Chemical Surface Preparation, Passivation, and Cleaning, Growth and Processing, Symp. B, Paper 3.1, Spring Mtg. of MRS, San Francisco, CA, April 12-16, 1992 and also in Semicon/Korea 91 Tech Proc., Seoul, Korea. Chapt...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[345] H.-S. Sohn, J.W. Butterbaugh, E.D. Olson, J. Diedrick, N.-P. Lee, MICRO 23 (5) (June 2005) 67. [346] M. Toda, S. Uryuu, in: J. Ruzyllo, T. Hattori, R.L. Opila, R.E. Novak (Eds.), Electrochemical Society (ECS) Symposium Proceedings: 2003-26 Eighth International Symposium on Cleaning Technology in Semiconductor De...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[356] M. Boumerzoug, in: IEEE/SEMI Advanced Semiconductor Manufacturing Conference (ASMC), 2014, p. 330. [357] F. Pipia, A. Votta, E. Ravizza, S. Spadoni, S. Grasso, S. Borsari, C. Lazzari, M. Alessandri, Solid State Phenom. 187 (2012) 227. [358] F. Pipia, A. Votta, A.C. Elbaz, S. Grasso, E. Ravizza, S. Spadoni, M. A...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[368] D. Bhattacharyya, P. Muralidhar, M. Conrad, Solid State Phenom. 255 (2016) 168. [369] H. Habuka, S. Ohashi, T.A. Tsuchimochi, T. Kinoshita, J. Electrochem. Soc. 158 (5) (2011) H487. [370] D.S. Mui, E.H. Lenz, C. Cyterski, K. Venkataraman, M. Kawaguchi, IEEE Trans. Semicond. Manuf. 24 (4) (2011) 552. [371] B.K. ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Chapter Outline 2.1 Wafer Contamination | 88 | | | | | |-------------------------------------------|------------------------------------------------------------|-----|---------|----------------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2.1.2.1 | Statistical Yield Models | 93 | | | | | 2.1.2.2 | Defect Size Distribution | 95 | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2.2.1.2 | Effects of Particulate Contamination | 104 | | | | | 2.2.2 | Metallic Contamination | 106 | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Handbook of Silicon Wafer Cleaning Technology. https://doi.org/10.1016/B978-0-323-51084-4.00002-2 Copyright © 2018 Elsevier Inc. All rights reserved. 87
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2.2.3.2 | Bases | 121 | | | | |------------|---------------------------------------------|-------|-------|---------------|-----| | 2.2.3.3 | Condensables | 121 | | | | | 2.2.3.4 | Dopants ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2.3.4 | Ion Implantation | 135 | | | | | 2.3.5 | Plasma Reactors | 136 | | | | | 2.3.5.1 | Particle Contamination | 136 | | | | | 2.3.5.2 | Post-etc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.1 Wafer Contamination The criterion for a substance to be considered a contaminant is that it causes uncontrolled variations in the electrical performance of the device or in the device fabrication process. Contamination may originate from the wafer itself, from the cleanroom, from process tools, or from process ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.1.1.1 Classification According To Detection Method Many analytical tools are available to detect the presence of contamination on a wafer, and normally a contaminant can be detected with more than one type of analysis. For a review, refer to Chapters 11e13. The following types of contaminants are distinguished: M...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Surface defectivity: defectivity associated with the roughness of Si or film surface or the line edge roughness. Typically, optical methods or atomic force microscopy and associated techniques are used to detect these types of defects. Atmospheric molecular contamination (AMC) and moisture: contamination that has mole...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![108_image_0.png](108_image_0.png) ## 2.1.1.2 Classification According To Material Technological progress has resulted in a diversification of materials that are used in the fabrication of silicon devices. Initially, the materials were limited to Si and the dopants necessary to control its semiconducting properties,...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
As the wafer surface of the device becomes more complex, for example, when the surface is patterned and multiple materials are exposed or when gate-level features are exposed, the range of acceptable chemical cleaning options becomes more limited. If the contamination consists of the same material as the substrate, th...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Chapter 3 discusses this method in more detail. ## 2.1.1.3 Classification According To Force Of Adhesion The force of interaction between contamination and a substrate determines if, and how strongly, the contamination will adhere. The forces that play a role in this interaction can be used in a classification scheme...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.1.1.4 Classification According To Size Contamination on wafer surfaces may have characteristic dimensions that span several orders of magnitude with respect to the size of the particle or concentration of the contaminant. Molecular contamination involves both atoms and molecules. These contaminants may be physica...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
As in any manufacturing business the profitability is directly related to the cost of processing and to the number of devices that can be produced. At the same time, the performance of the chips is linked to their selling price. Failing devices can often be traced to uncontrolled or unwanted fluctuations in the fabrica...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The determination of "critical contamination levels" is therefore not straightforward. ## 2.1.2 Yield Models, Reliability, And Relationship To Defectivity Models are used within the IC manufacturing community to relate defectivity to the device yield. Yield is defined as the fraction of devices that are functional at...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Fundamental to most yield and reliability modeling is the assumption that the defects are small compared to the device area. Large defects such as scratches are typically not considered, possibly because they are relatively rare and usually not random. ## 2.1.2.1 Statistical Yield Models Poisson distribution: This mo...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Weibull distribution: The Weibull distribution is widely used to describe the lifetime distributions of systems that fail due to the "weakest link." The cumulative probability function F(t) is expressed as: $$F(t)=1-\exp\biggl({\frac{t-\gamma}{\eta}}\biggr)^{\beta}$$ $$(2.1\text{-}4)$$ $$(2.1{\mathsf{-5}})$$ b(2.1-4) ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Using Eq. (2.1-1), and considering that $${\mathrm{yield}}=1-F$$ $$(2.1{\cdot}6)$$ yield ¼ 1 - F (2.1-6) it is shown that $$\ln[-\ln(1-F)]-\ln A=\ln D$$ $$(2.1{\bar{-}}7)$$ ln½lnð1 - FÞ - ln A ¼ ln D (2.1-7) where A is the device area and D is the defect density. This means that the Weibull distribution scales with d...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
This does not necessarily correspond to the physical particle size, since defects are not always particles. To describe the defect size dependence, the defect density D(d) is defined as a function of defect size d. Often a power law is used of the form $$D(d)=D_{0}\biggl({\frac{d_{0}}{d}}\biggr)^{p}$$ $$(2.1{\cdot}8)...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.1.2.3 Effective Area Some areas of a device are more sensitive to defects than others. For this reason, an effective chip area Aeff(d) can be defined that represents the area of the chip that is sensitive to defects of size d. For defects smaller than the critical defect size Aeff is assumed to be zero. For large...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$${\frac{d C_{i}}{d t}}+{\overrightarrow{\nabla}}\cdot{\overrightarrow{J}}_{i}=S_{i}$$ $$(2.1\!\cdot\!10)$$ $$(2.1\!\cdot\!11)$$ The contaminant flux J !i in any direction results from diffusion, convection, and the effects of an electric field on a charged species and may be described based on the NernstePlanck equat...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In the case of Eqs. (2.1-10)e(2.1-12), the term "reaction" refers to the partitioning of i onto the wafer from solution, whether by physical adsorption or by chemical reaction, and to the partitioning of i off the wafer surface into solution. If the contamination process is reaction rate limited, then the rate of trans...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$$L_{\mathrm{diff},i}={\sqrt{2D_{i}\Delta t}}$$ $$(2.1\!\cdot\!13)$$ 2DiDt p (2.1-13) For a given change in ss,i, Eqs. (2.1-10)e(2.1-12) indicate that there will be a corresponding change in Ci. The ratio of Dss,i to DCi defines a hypothetical equivalent layer thickness based on the contamination deposited on or remov...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.1.3.2 Contamination Transport Through Liquids Wafers come into contact with liquids during chemical mechanical polishing (CMP), and during cleaning, drying, and etching steps. In a static immersion tank !u ¼ 0 (Eq. 2.1-11). The transport of contaminants occurs by diffusion and is driven by gradients in the contam...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$$\delta\sim S{\sqrt{\frac{p\cdot x}{u_{0}}}}$$ $$(2.1\!\cdot\!15)$$ r(2.1-15) with n the kinematic viscosity, u0 the liquid velocity away from the wafer, and x the position on the wafer, measured downstream from the edge. The boundary layer can be estimated to be several mm under typical processing conditions [33]. Wi...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Only at very high pH, >10, does the SiO2 dissolve by forming soluble silicates. Hydrogenated Si surfaces, as shown in Fig. 2.1-3, can be obtained by exposure to nonoxidizing environments, such as hydrogen fluoride (HF), caustic solutions with low oxidation potential (e.g., Si polishing), or H2 ambient during high-temp...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
with Kþ and K- the protonation and deprotonation constants. Due to this protonation/deprotonation behavior the silicon surface will bear a negative or positive surface charge s0 [39]: $$\sigma_{0}=q N_{0}{\frac{\left[\mathrm{SiOH}_{2}^{+}\right]-\left[\mathrm{SiO}^{-}\right]}{\left[\mathrm{SiOH}_{2}^{+}\right]+\left[\...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$$[H^{+}]=[H^{+}]_{\mathrm{bulk}}\,\exp\left[-\frac{q\varphi}{k T}\right]$$ $$(2.1\!\cdot\!19)$$ i(2.1-19) Using the Poisson equation, and assuming that only monovalent ions are present, the integrated charge in the diffuse layer per unit area is $$\sigma_{d}=\frac{2\varepsilon}{L_{D}}\frac{kT}{q}\sinh\biggl{[}\frac{q...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.2 Behavior And Impact Of Contamination 2.2.1 Particle Contamination 2.2.1.1 Origins of Particle Contamination Particles are always present in the atmosphere. Outside cleanrooms, particulate contamination may be visible as smog, fog, or dust, that have varying origins, such as emissions from human activities, dese...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In aerosol science, experimental particle size distributions often closely follow a lognormal size distribution. However, it has also been observed that in many cases a power law with parameter a can approximate particle size distributions: $$\mathrm{d}N=f(d)\mathrm{d}d\quad{\mathrm{with}}\quad f(d)={\frac{C_{0}}{a d_...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$\mathbf{C}_{n}=35.31n\left(\frac{0.5}{d}\right)^{2.2}$ $$(2.2\mbox{-}25)$$ 2:2(2.2-25) where n is the allowed number of particles per ft3 at 0.5 mm particle diameter. The factor 35.31 converts the US standard to SI units (particles per m3). ![121_image_0.png](121_image_0.png) A comparison of the ISO standard and the...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The detrimental impact of particles is one of the reasons microelectronic devices are fabricated in the controlled environment of a cleanroom. Particle count is one of the most important criteria for process control. At the same time, there is surprisingly little experimental evidence for the detrimental impact of part...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The impact may be a function of particle material and size, and layer thickness, composition, and deposition method. ## 2.2.1.2.2 Back Surface Particles The impact of back surface particle contamination is difficult to determine when processing single-side polished wafers. The main reason is that the roughness of the...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
An often-quoted effect of back surface particles is the formation of "hot spots" during lithographic pattern definition [50,52,53]. The vacuum that holds the wafer on the chuck causes a local deformation of the chuck, particle, and wafer due to the presence of the particle. The local forces are so large that a plastic ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The feasibility of this mechanism is illustrated by common practice: cycling a number of dummy wafers through the handling system can reduce handlinginduced contamination. Back surface contamination occurs not only in the form of particles; both metallic and organic contaminants are also detrimental. Copper, in partic...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The use of Pourbaix diagrams is subject to the condition that complexing species are not present and insoluble salts are not formed. Obviously this is not always true. Table 2.2-1 lists the solubilities of some sparingly soluble metal hydroxides and metal fluorides. These salts will precipitate if their concentration i...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.2.2.2 Metallic Ion Exchange Reactions When SiOx is exposed to an aqueous chemistry, an equilibrium is established between protonated and deprotonated silanol (SiOH) groups. The effect on surface charge has been discussed previously in Section 2.2.1.3. When metallic cations are present in the solution, they not on...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| TABLE 2.2-1 Solubility Products of Sparingly Soluble Metal Hydroxides and Fluorides [64] Maximum Dissolved | Maximum | | | | | | | | |--------------------------------------------------------------------------------------------------------------|---...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Co | Co(OH)2 | 5.92 1015 | >1000 | >1000 ppm | 35 ppb | | | | | Cr ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Mn | Mn(OH)2 | 2.00 1013 | >1000 | >1000 ppm | 1 ppm | | | | | Ni ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Included are calculated maximum levels for some typical conditions (compiled by authors). For HF, a dissociation constant of 7.2 10e4 was used. Used with permission from CRC Press Inc. SECTION j I Introduction and Overview TABLE 2.2-2 Overview of Metal Complexes and Their Formation Constants [54]
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| [54] Metal | Hydroxide | Log K | Ammonia, Fluoride, and Chloride | Log K | |--------------------------------------------------------------------------------------------------|--------------|---------------|-----------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2þ | 11.8 | | | | | Cu | [Cu(NH3)4] | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| 2e | 18.3 | | | | | Ti | [Ti(OH)4] | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The selection was made based on the criterion that more than 0.01 wt% of the metal ions would be complexed with a ligand concentration of 1.0 M and a total metal concentration of 1.0 10-8 M. R.M. Smith, A.E. Martell, Critical Stability Constants, in: Inorganic Complexes, vol. 4, Plenum Press, New York, London, 1976. ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Fig. 2.2-9 shows schematically two different metal redox systems M1 and M2 with their respective redox levels E0M1 and E0M2. Fig. 2.2-10 shows the position of the conduction and valence band edge of the Si substrate in contact with the dilute HF solution and the redox potential of the different noble metal redox system...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![130_image_0.png](130_image_0.png) of the Cu2þ ions, while for n-type Si photogenerated holes are consumed by the Si oxidation. Thus for both p- and n-type Si wafers, the Cu outplating is enhanced under illumination, as shown in Fig. 2.2-11 [58]. Measures can be taken, such as adding complexing agents to the solution...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$$\mathrm{Si}+2\mathrm{HF}+2\mathrm{H}^{+}\leftrightarrow\mathrm{SiF}_{2}+2\mathrm{H}^{+}$$ $$(2.2\text{-}29)$$ Si þ 2HF þ 2Hþ4SiF2 þ 2Hþ (2.2-29) The unstable SiF2 reacts further with HF and/or H2O molecules to form SiF26 . ## 2.2.2.4 Behavior Of Metallic Contamination Whereas particulate contamination is often con...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Metallic impurities may dissolve in the Si and diffuse to sensitive device areas [65,66]. Fig. 2.2-12 shows the diffusivities of numerous metals in Si. Among the metals with the highest diffusivities, the transition metals (Cu, Fe, Ni, Co, Cr, and Mn) are most relevant for processing of silicon devices. Other metals (A...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Metals in Si have a finite solubility that decreases with decreasing temperature, as shown in Fig. 2.2-13. If the metal concentration exceeds the solubility, the dissolved metals will precipitate, usually by silicide formation. Energy is needed for precipitation due to the volume expansion; for example, ![131_image_0...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The removal of metallic solutes from certain regions in the substrate is also known as "gettering." Apart from gettering by defects, impurities can also be gettered in regions of the device that have a higher solubility for the impurity than the bulk Si, such as highly doped regions and interfaces to polysilicon and Al...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![133_image_0.png](133_image_0.png) of these ions, especially Naþ and Kþ, are extremely high and detrimental to devices, as outlined in Section 2.2.2.5. Low-k materials exhibit similar behavior to SiO2, except their interaction with contaminants may be different. As a result, some metals may be present as ions in low...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.2.2.5 Effects Of Metallic Contamination Metallic contamination can have detrimental effects on device performance. This may be caused by incorporation of the contaminants into sensitive device regions, or by loss of process control induced by the contaminants. ## 2.2.2.5.1 Effect On Process Control The presenc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![135_image_0.png](135_image_0.png) ## 2.2.2.5.2 Bulk Silicon Defects The presence of defects in bulk Si disturbs the periodicity of the lattice and thus introduces energy levels that are located within the bandgap, which can enhance the generation and recombination of minority carriers. Generation can be observed if...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Recombination can be observed if excess carriers are injected. With n and p the electron and hole concentrations, and assuming low injection conditions (concentration of minority charge carriers remains lower than the concentration of majority charge carriers), the so-called "ShockleyeReade Hall" recombination lifetime...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![136_image_0.png](136_image_0.png) ## 2.2.2.5.3 Defects In Dielectrics Gate dielectrics are characterized by their excellent insulating and capacitive properties. Metallic impurities on the wafer surface, prior to gate dielectric formation, usually degrade these properties by locally reducing the tunnel barrier or b...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
(2.2-29) and (2.2-31). However, surface generation and recombination is generally more complex than bulk generation and recombination [95]. Whereas bulk defects usually exhibit distinct energy levels within the band gap, surface defects introduce a broad distribution of interface state defect levels. Moreover, the gene...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
A special class of defects consists of ionized metallic impurities in dielectrics, which can drift under influence of an electric field. Best known are Naþ, Kþ, and Liþ contamination, usually of human origin or from packaging materials. In state-of-the art cleanroom facilities, these contaminants largely have been elim...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In SEMI Standard F21-95 [107], different types of AMC are distinguished: Acids: corrosive materials whose chemical reactions are those of electron acceptors. Bases: corrosive materials whose chemical reactions are those of electron donors. Condensables: chemical substances capable of condensation on a clean surface. ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Also, trace levels of HF may end up in the air recirculation system and give rise to dopant contamination, as discussed in Section 2.2.3.4. In the case of acid, base, and condensable contamination, it is often observed that deposition on surfaces causes hazing, especially in the presence of moisture [110e112]. This ph...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Since these resists rely on the photogeneration of acids, the presence of as little as 10 ppb of amines in the cleanroom air can cause its diffusion into the photoresist and neutralization of the photogenerated acids [113]. The result is the so-called "T-topping" or "skin-formation" of the photoresist, as shown in Fig....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Although the precise mechanism of adsorption is not understood, it is assumed that condensables with low boiling points (below 150C) or with low molecular weights are of little importance because their residence time on the surface is relatively short [127]. Several other factors are known to play a role as well. A the...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| TABLE 2.2-3 Examples of Common Airborne Molecular Contaminants and Their Effects on Wafers [134] Boiling Vapor Chemical Formula CAS No. amu Point (C) Pressure (Torr/25C) | Application | Effects | | | | | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Nitric acid | HNO3 | 7697-37-2 | 63 | 83 | 63 | | | | | | Bases | Hexamethyl disilazane | HMDS | C6H19NSi2 | 999-97-3...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Condensables | Dioctyl phthalate | DOP | C24H38O4 | 117-81-7 | 391 | 387 | 1.4 107 | Plasticizers | Hydrophobie wafer surface, poor layer adhesion | | Diethyl hexyl | DEHP | | |...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| TABLE 2.2-3 Examples of Common Airborne Molecular Contaminants and Their Effects on Wafers [134]dcont'd Boiling Vapor Chemical Formula CAS No. amu Point (C) Pressure (Torr/25C) Application | Effects | | | | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Stearic acid | C18H36O2 | 57-11-4 | 285 | 383 | 7.2 107 | | | | | | Phenol | C6H6O | 108-95-2 | 94 | 182 | 0.35 | | ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
may occur if the temperature ramp-up is conducted in an inert environment, even with minimal amounts of C left on the wafer, or if the organic contamination is not completely burned off or vaporized during rapid thermal processing [110,131]. This can affect the gate oxide integrity [125,131,135,136]. Other detrimental...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.2.3.5 Moisture Relative humidity is defined as the ratio of the actual H2O vapor pressure, p, over the saturation vapor pressure, ps, at the prevailing temperature: $$R H={\frac{P}{p_{\mathrm{s}}}}$$ $$(2.2\mbox{-}35)$$ RH ¼ pps(2.2-35) where RH is the relative humidity. The saturation vapor pressure of water a...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![144_image_0.png](144_image_0.png) 300e400C. Partially dehydroxylated SiO2 will slowly rehydroxylate when exposed to H2O vapor. Low-k dielectric materials are usually hydrophobic, and thus, not much moisture is adsorbed. However, after exposure to plasma, as in the case of photoresist stripping, polar silanol groups...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Chapter 8 discusses the process of repairing and sealing the low-k material. ## 2.3 Sources Of Defects And Contamination In the following sections, we will discuss several media and process tools that can be sources of contaminants and defects. ## 2.3.1 Cleaning-Related Defects 2.3.1.1 Megasonic Damage Megasonic en...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.3.1.2 Transient Effects During Rinsing When a substrate is transferred from a cleaning mixture to a rinse bath, it carries over a chemical layer that contains cleaning agents and possibly contaminants. When the wafer is immersed in pH-neutral water, the carry-over layer changes from acid or alkaline pH to neutral...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.3.1.3 Drying Residues In the last stage of the drying process, H2O evaporates and leaves behind any nonvolatile residues that were present in the evaporating H2O layer. In the case of spin-drying, the thickness of this water layer is of the order of 5 mm, whereas for Marangoni drying it is two orders of magnitude...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
$${\frac{F_{\mathrm{cap}}}{l}}={\frac{\gamma\,\cos\,\theta}{s}}$$ $$(2.3\text{-}38)$$ where q is the contact angle, g is the liquid surface tension, and l and s are the length and spacing of the lines, respectively. If the capillary forces on both sides of the lines are in equilibrium, and if the spacing varies, or if...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Substrate charging can be controlled in a number of ways. Air ionizers are able to neutralize substrate charge, but there have been concerns about their contribution to particle contamination levels. Humidity provides a conducting path to ground by forming a layer of adsorbed moisture on surfaces; however, it also incr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The impact of roughness on devices continues to be a concern. However, it should be noted that many studies on the topic artificially increase the roughness to above 1 nm RMS (root mean squared) values, which is large compared to what is typically required in production lines [20]. It is known that the tunnel current t...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 2.3.1.7 Corrosion Corrosion of metal lines is a widespread problem for microelectronic device fabrication [16]. It is an electrochemical reaction, and thus involves both oxidation and reduction reactions. Corrosion proceeds due to a potential that exists between two metal regions; this may be a galvanic potential o...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Possible oxidation reactions at the anode are $$\Delta G=-n F U$$ $$\begin{array}{l}{{\mathrm{Mt}\!\rightarrow\!\mathrm{Mt}^{n+}+n\mathrm{e}^{-}}}\\ {{\mathrm{Mt}+n\mathrm{OH}^{-}\!\rightarrow\!\mathrm{Mt}(\mathrm{OH})_{n}+n\mathrm{e}^{-}}}\\ {{\mathrm{Mt}+n\mathrm{H}_{2}\mathrm{O}\!\rightarrow\!\mathrm{MtO}_{n}+n\mat...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Metal deposition is undesirable because it can cause short circuits between metal lines, whereas formation of soluble metal hydroxides can cause open circuits. The charge transport required for these reactions occurs in the H2O layer that is adsorbed on the surface. Moisture, therefore, has a strong impact on the corr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress