| TABLE 7.2-2 | Typical High-Dose Implant Photoresist Strip and Clean | |---------------|---------------------------------------------------------| | Processes for Downstream or Inductively Coupled Modulesdcont'd MW plasma 2000 W 1000 W 800 W Radio frequency (RF) 75 W Off Off bias plasma Pressure 5 m Torr 1.0 Torr ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The residue that may be present on an inadequately cleaned wafer is shown in Fig. 7.2-9. The typical residue is (1) "popping" residue, unreacted photoresist, (2) post-implant species residue, and (3) sputtered SiO2 residue. Using the appropriate plasma strip and clean process is important, to target the removal of thes...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Low-temperature crust removal, typically at a temperature lower than the photoresist hard-bake post-develop temperature, is used during the crust removal step to prevent the photoresist from "popping." The bulk strip step ![413_image_0.png](413_image_0.png) then can revert to the higher temperature to achieve a fast ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.2.4 Post-Etch Resist Stripping And Cleaning 7.2.4.1 Removal Of Polymers Polymer formation occurs at many steps in the manufacturing of IC devices. Some plasma etch processes purposely deposit polymer to protect the sidewall etching that erodes the critical dimension (CD). High-energy and high-dose ion implantati...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Although plasma stripping can effectively remove photoresist, removing residue can be difficult. The difficulties arise when the residue is inert to the plasma and additives such as F-containing molecules must be added to remove the fluorocarbon polymer or the silicon sidewall polymer. The F-containing gases not only r...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![417_image_0.png](417_image_0.png) Fig. 7.2-13. The hardmask may be kept in place, for example, if it is composed of SiO or SiN or may be removed if it is TiN or an etchable material such as amorphous carbon. Amorphous C may be simply removed with an O2 plasma similar to that used in stripping bulk photoresist. When...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![418_image_0.png](418_image_0.png) polysilicon gate after etching but before stripping and cleaning. The polymeric residue on the sidewall is clearly delineated as is the bottom antireflective coating (BARC) and the photoresist. Fig. 7.2-12B shows the top view of the polySi gate after strip but before cleaning; the re...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The sidewall residue remains after the plasma strip process and must be removed to prevent unwanted contamination of the polysilicon or gate oxide and to allow adequate adhesion of the next deposited layer. Because the sidewall is mainly composed of Si and SiO2, etching the sidewall will also etch the gate dielectric a...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Surface oxidation of tungsten during photoresist stripping can present serious CD changes in the gate electrode. Indeed, a remote O2 ICP used to strip photoresist from tungsten surfaces at or below 300C oxidized the tungsten surface [52]. The extent of tungsten oxidation to form WO3 increased with increasing temperatur...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Downstream Microwave (MW) Module (B) [51] Process A: Post-gate Stripping and Cleaning Process Step 1 Gas Stabilization | Step 2 Plasma Stabilization | Step 3 Photoresist Strip | Step 4 Residue Removal | Step 5 Chamber Purge | | |------------------------------------------------------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Pressure | 1.5 Torr | 1.1 Torr | 1.1 Torr | 1.1 Torr | 1.5 Torr | | Temperature ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| MW plasma | 900 W | 1100 W | | | | | Pressure ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
SECTION j III Dry Cleaning Processes 402 Similar concerns exist for unwanted silicon oxidation as the gate oxide layer thickness is reduced for advanced devices. That is, photoresist removal after gate stack etch exposes the remaining gate oxide in the adjacent stack regions to an O2-based plasma, which can increase th...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Fig. 7.2-12C and D shows cross-sectional SEMs of the polymeric residues on the sidewalls of a contact and via. The contact SEM shows the feature before the stripping and cleaning steps, and polymer is clearly visible on the sidewall and the bottom of the feature. The resist is reticulated and dehydrated and likely has ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![422_image_0.png](422_image_0.png) ![422_image_1.png](422_image_1.png) such as CF4, NF3, and SF6, either with an O2-based or a H2-based plasma. The F-containing gases are able to etch the polymer, by forming volatile CxFy species, and can also etch any embedded Si in the polymer. However, because of the presence of ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Chapter 10 discusses surface chemistry of Al. Many researchers have investigated the use of H2-based plasma formulations for various applications such as cleaning Si before epitaxial deposition, as discussed in Section 7.2.6. More recently, to clean the polymer that is formed during the via etching process, interest h...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The dual damascene etching and stripping process flow is shown in Fig. 7.2-20, where the interlevel dielectric film is a low-k material. The cleaning method required when low-k dielectrics are present is dependent on the type of low-k material and the integration scheme used in the formation of the dual damascene struc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![425_image_0.png](425_image_0.png) ![426_image_0.png](426_image_0.png) to 275C increased the removal rate. N2 additions to the H2 plasma showed little effect on the stripping rate, but the damage depth to the ULK increased substantially as the N2 content increased. After patterning ULK layers using a C4F8 plasma, mo...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Cleaning of the low-k dual-damascene structure requires successful removal of the photoresist and BARC films. No bowing or other modification of the via and trench profile, no change to the CD of the via and trench feature, and no alteration of the dielectric constant from plasma damage may occur. The sensitive low-k m...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Plasma recovery of the dielectric constant value after stripping and cleaning has been reported, by using a reducing [66] or by a CH4 plasma [67]. Whether such processes recover the low-k properties by removing H2O embedded in the material or by substitution of O in the CDO with H is unclear at present. Stripping and ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In addition, inert gases such as He or Ar may be added in place of N2. Temperatures used to strip and clean low-k materials vary depending upon the specific process requirements. High temperature removes photoresist and residues rapidly and may deter the condensation of H2O, while low temperatures may limit the damage...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Removal of the photoresist after the etching process is sometimes performed in situ at the same time that the etch chamber is being cleaned of the built-up organic residue from the stripping process. However, transfer of the wafer to an ex situ plasma strip system is typically performed for most layers in IC manufactur...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[76], who reported that the gas chemistry selected affected the via profile. As device dimensions and film thicknesses continue to decrease, etch selectivity to underlying films and substrates becomes increasingly important. Such concerns can be addressed by ensuring spatial uniformity of photoresist or residue remova...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Although most ALE investigations have considered Si removal, there have been other materials studied, including polystyrene [81]. In this study, the polystyrene surface was treated with O2 to allow adsorption, residual O2 was then evacuated from the chamber, and reaction products subsequently desorbed by a loweion ener...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
An alternative to residue removal in a plasma chamber is to modify the resist and residue, without stripping it completely, then using a wet cleaning formulation to remove the modified resist and residue to prevent damage to the sensitive dielectric material [82]. In this case, ion bombardment and vacuum UV is used to ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In some cases, as reported by Christaud et al. [84], after etching and stripping, wafers are transferred to the plasma cleaning system. The polymeric residue is removed using CF4 and forming gas (N2/4 vol% H2) at a temperature of 75C. Finally, the wafer is processed through a DIW rinse to remove chloride-embedded surfa...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.2.6 Pre-Epitaxial Deposition Cleaning Epitaxial deposition is used to create an epitaxial (epi) layer (homoepitaxial or heteroepitaxial), such as Si, Ge, SiGe, SiC, or SiGeC on the Si substrate. The applications include epitaxial Si or SiGe on Si substrates for silicon on insulator, epitaxial wafer formation, and...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
There are many ways to effectively clean the Si surface before epi deposition. Chapter 6 discusses passivation of the Si surfaces using HF in the gas-phase and UV-assisted treatments. Another method uses a hightemperature H2 bake (>900C), which reacts with surface C and O to form volatile products. Typically, CVD epi d...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The temperature should be low during epi deposition. The necessity for low-temperature epitaxial technology is because of the low thermal budget required to maintain doping profiles for shallow channel structures [98]. Plasma processes allow a higher reactivity at lower temperatures. For bulk epi deposition, it is not...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Various analytical methods have been used to evaluate Si surfaces after cleaning and epi growth. For instance, XPS is a frequently employed technique; additional methods include spectroscopic ellipsometry for process optimization, discussed by Fo¨rster et al. [106], analysis of the properties of the strain in Si after ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
After the remote H2 plasma clean process, the Si surface is structurally well ordered, free of O and C, and is H terminated. This allows low defect density deposition of both Si and SiGe, resulting in ultra-low temperature Si homoepitaxy at temperatures as low as 150C [114]. It is important to remove the H on the Si su...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[114] showed that Si surfaces were more resistant to oxidation and demonstrated the effectiveness of H2 plasma treatments for removing O from oxidized surfaces. The experiment showed that 10 h after a modified RCA treatment, substantial C and O appear on the surface of a Si wafer when exposed to atmosphere even though ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.2.7 Pre-High-K Deposition And Oxidation Plasma Cleaning Cleaning of the silicon surface before high-k deposition is usually performed with an HF vapor and UV clean. However, remote H2-based plasmas are also effective at removing unwanted oxides and preparing the surface for deposition in the same manner as pre-ep...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Sputtered metals from the preceding etch process or from the etch reaction and post-etch polymeric residues can also be present. Wet chemical cleaning processes usually precede the pre-deposition cleaning step. These wet cleaning processed are discussed in Chapter 4. One method of pre-deposition cleaning is sputter et...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Cleaning Cu with a H2 downstream source is disclosed in US patent 6,905,965 [121]. First, an F-containing plasma is used to remove SiO2 and fluorocarbon polymers, then an in situ reducing gas is used to convert the CuO to Cu without sputtering the Cu sublayer. Table 7.2-5 shows the recipe used for this process. This pr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
However, stress migration of the Cu can be induced because of an aggressive Ar sputter etching pre-cleaning step [123]. ## 7.2.9 Other Applications Of And Approaches To Plasma Cleaning Soft etching of a surface previously exposed to a plasma is another surface conditioning method. These processes remove the thin dama...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Atmospheric pressure plasma jet cleaning is used for various industrial applications such as removing paint and cleaning metal surfaces of organic contamination [126,127]. Arc plasma jet cleaning of the Si surface before CoSi2/Si contact formation has been reported by Ya et al. [128]. The plasma jet cleaning improves S...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.2.10 Cleaning And Conditioning Plasma Chambers The plasma chambers used for etching, deposition, and cleaning can become coated with the byproducts of the various reactions performed. This deposited material can detrimentally affect the process by lowering removal rates or deposition rates and also create particl...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| TABLE 7.3-6 | Overview of Plasma Parameters for Stripping and Cleaning | | | |------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Low-energy ion bombardment, more chemical effects | MW downstream or inductively coupled plasma (ICP) | Oxidizing: O O3, | Prevents | | N2O ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Low | Power Ranges | Flow Ranges | Low | | >100 ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
and repeatable plasma. The key parameters that control the plasma and contribute to the results of the process are outlined in Table 7.3-6. ## 7.3.2 Overview Of Physical And Chemical Mechanisms For Stripping And Cleaning Remote plasma cleaning of surfaces during the manufacture of ICs has been successfully implemente...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Momentum transfer (sputtering) by ions physically dislodges residue and photoresist and breaks surface chemical bonds, and the reactive atoms and radicals chemically react with residue or photoresist to form volatile or soluble products. Higheatomic weight atoms such as Ar, are especially useful for sputtering, whereas...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Byproducts are produced during the photoresist stripping process, some of which are volatile; however, some of the byproducts are incompletely reacted species that deposit on the walls and vacuum ports of the chamber. After a critical thickness of residue builds up on the chamber wall, the film starts to peel and flake...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.3.3.1 Chemistries For Photoresist And Residue Removal Various plasma stripping and cleaning chemistries currently exist for removal of photoresist and residues. This section will cover the most common chemistries used for stripping and cleaning. The chemistries used for photoresist stripping and cleaning are comp...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![441_image_0.png](441_image_0.png) result, care is usually exercised during IC manufacturing to avoid this undesirable occurrence. In addition to photoresist, other materials are used in the lithography process. Before photoresist is applied to the wafer, a priming agent such as hexamethyldisilazane is usually coate...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Oxidizing Chemistries: Oxidizing chemistries are typically composed of O2 plus a carrier gas and additives. The oxidizing species can be O2, H2O, or N2O or other gases containing an O atom. Because photoresist is composed of hydrocarbons, the O2 plasmas generate O, which easily reacts with this film to form volatile by...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The stripping rate achieved by using O2/N2 chemistry is higher than that attained with the H2/N2 chemistry, under similar process conditions. Researchers have shown that the difference becomes more significant at high temperatures [142]. The measured activation energy for photoresist strip using O2/N2 plasma is w10 kc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
However, forming gas (4e10 wt% H2 in N2) is usually a safer alternative than the use of H2. Furthermore, the formation of NH radicals in forming gas plasmas, which yields eCNH moieties as reaction products, appears to assist the decomposition and volatilization of photoresist materials [140]. There are limitations when...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Additives Chemistry: Additives for stripping and cleaning can be F-based. Inert gases are also added in some cases. Although H2O is considered an additive, as is H2 in an O2 plasma, or O2 in a H2 plasma, these are actually components of the reaction process. Additives, such as CF4, have been shown to modify the main c...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Additives may also be inert. Helium, Ar, and N2 are the most common. If increased ion bombardment is needed, Ar is a good choice; if increased cooling is needed, He is a good choice, but high-energy photon emission from these plasmas may also affect underlying layers. However, these gases are electropositive and may af...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Copper films that have been oxidized by wet processing steps and passivated with organic complexing agents can be cleaned through the use of H-based plasma processes, and then passivated with H2, although etching of Cu in H2 plasmas at low temperatures can occur readily [145,146]. The Cu surface can subsequently be reg...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Although temperature effects can be beneficial to enhance photoresist removal rate, it is important to consider all films that will be exposed to the plasma and determine if certain temperature regimes alter the etch selectivity. For instance, the rate of H2-based stripping of 193 nm resist materials increases substant...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.4 Plasma Stripping, Cleaning, And Surface Conditioning Equipment There are several types of commercially available plasma process systems used for resist stripping and cleaning. The most common reactor types include inductively coupled sources and both remote (downstream) and biased (parallel plate) RF and MW dis...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Multiple wafers (batch process) are placed in a holder that is generally isolated from the plasma by a perforated (often Al) etch tunnel which serves as a Faraday cage to shield the substrates from ion and electron bombardment. The tunnel improves temperature and thus etching rate uniformity across the batch of wafers...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
As device sizes decreased and aspect ratios >3 became the norm, anisotropic etch profiles were required. In the late 1970s, parallel plate reactors became the workhorse for plasma-assisted pattern definition [93,155]. Because substrates reside within the plasma, resist stripping and cleaning in such reactor configurati...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Batch (multiple wafer) processes were used initially in plasma processing to maximize production throughput. The continuing increase in wafer size along with the improved process control needed to achieve within-wafer and wafer-to-wafer uniformity at small feature sizes resulted in single-wafer approaches to etching an...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.4.2 Remote Plasmas: Downstream Generation Typically, in a remote plasma process, a reactant gas is introduced through the plasma tube where it is ionized and/or dissociated by the applied plasma power. Operating pressures are usually in the range of 100e1000 mTorr. Reactive species such as atomic O generated by ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Elbow bends in the downstream reactor system are also important because one 90-degree bend is usually sufficient to eliminate charged species and unwanted photons that may cause electrical damage to the wafer. In addition, materials of construction for the gas distribution showerhead and the geometrical configuration o...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The frequency of the power for plasma generation was not clearly defined when remote plasma photoresist stripping was first introduced [158,159]. The frequencies are now based on Federal Communication Commission acceptable ranges that do not interfere with communications and are outlined by standards set by the Industr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Sputtering of the chamber material on the wafer is a concern anytime highenergy ions are used for etching. Aluminum contamination is of particular concern because the majority of the process chambers are composed of aluminum or alumina. Where possible, plasma systems used for IC manufacturing should avoid stainless ste...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
However, sapphire tubes can be cooled to prolong their lifetime. One-piece sapphire tubes are preferable because of the manufacturing issues caused by creating the tubes. In some cases, a 90-degree bend is included in the plasma tube to eliminate the need for baffles to prevent direct ion bombardment and line-of-sight ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
There are two major issues for MW downstream strippers in the production environment. The main issue is high cost of the MW generator quartz tube consumable. Because of the erosion caused by the plasma generation, the tube must be replaced frequently. The secondary issue is that the resist stripping rate in an MW downs...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
There are two different types of ICP systems. The first type is where the plasma has direct contact with the wafer to form a plasma sheath, plus an optional RF bias to control ion energy. In this case there is no major difference between an ICP plasma etching chamber and the stripping chamber. In this configuration, th...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
In this example, the wafer is in total darkness because the metal grid blocks all the UV originating from the plasma generation chamber. The Faraday shield placed between the RF coil and the quartz tube used for plasma generation is another key feature for advanced ICP systems. There are several purposes for this conf...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
![453_image_0.png](453_image_0.png) ![453_image_1.png](453_image_1.png) addition, one ICP supplier uses the conical chamber and coil configuration to produce reactive neutral species at varying distances within the chamber volume for nonion enhanced processing. This configuration provides uniform diffusion of the act...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
RIE addition also gives the ability to perform etching in the stripping and cleaning system. Etching of dielectric barrier films such as SiC or SiNx after the low-k dielectric post-etch clean eliminates the need to both remove the wafers from the stripping and cleaning system and transfer the wafers to an etch system f...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Hollow cathode plasma arrays have been proposed for photoresist stripping using H2/N2 mixtures [164]. This configuration generates a high-density uniform discharge in a 7:3 mixture of H2/N2 at 1.6 Torr, with a photoresist removal rate of 260 nm/min at 250C. ## 7.4.3.6 Other Plasma Sources Although it is beyond the sc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Ultrapure gas delivery is important to assure that contamination is not introduced into the reaction chamber. Stainless steel electropolished tubing is used because most gases do not react with this material. Corrosive gases, when used, typically employ double-walled, protective tubing. In addition, most gases are filt...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Movement of the wafer is designed to avoid scraping against surfaces; gentle movement of the wafer when placed on and removed from the platen eliminates unwanted contact that could generate particles. Movement in and out of the front-opening unified pod also is optimized so as not to generate particles from the movemen...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.4.5 Safety Care is taken to prevent accidental release of H2 into the atmosphere by the use of load locks, double-enclosed gas lines, and gas line interlocks. The percentage of H2 gas in reducing gas mixtures usually does not exceed 4 vol% to ensure safe operating conditions. However, higher amounts of H2 are bei...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Another safety concern is erosion of the quartz tube when using Fcontaining gases. The tube may thin to the point it becomes mechanically unstable. With <1% vol of F used, in general, is compatible with quartz tube. However, if higher F concentrations are used, ceramic tubes are recommended for better erosion resistan...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Plasma atmospheres supply chemically reactive species and ion bombardment for photoresist, residue, and contaminant removal. However, the complexity of the chemical and physical processes that occur during such processes is considerable. As a result, use of in situ plasma diagnostics to establish fundamental understand...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Highly sophisticated diagnostic techniques are available to investigate chemical species concentrations, ion fluxes, and ion energies, but such methods are typically incompatible with production systems. Instead, endpoint detection methods, which do not require nor necessarily generate fundamental understanding of the ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Stefani et al. shows an example of implementation of process monitoring of photoresist clearing times on a wafer-to-wafer basis using OES on a plasma stripping system [173]. Control of the process is made more difficult because prior processing steps such as ion implantation affect the properties of the photoresist mat...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Oxygen MW and RF plasma emissions have been studied [176e179] to assist in determining the optimum process parameters for photoresist stripping. The RF plasma generates more charged species, both Oþ and ee, than the MW plasma, which generates relatively more atomic O [182]. MW plasmas have been shown to have higher etc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
The wavelength of the light used to detect the endpoint is dependent on the reaction chemistry. Some of the reactive gases used in plasma stripping are very dilute and thus make detection of the byproduct or the reaction gas species very difficult. Also, downstream plasmas sometimes have few molecules in excited states...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Algorithms are set up to detect the endpoint based on the signal level and rate of change. ## 7.5.3 Laser And Optical Interferometry In addition to OES, laser interferometry, also called optical interferometry, is another endpoint technique for plasma stripping and cleaning. Interferometry is based upon detection of ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## 7.5.4 Residue Gas Mass Spectroscopy The gas molecules produced during the resist stripping or cleaning reaction that go into the exhaust can be used to detect an endpoint signal. In this case, some of the exhaust can be redirected into a small enclosed volume. Once enclosed, a small plasma source is used to strike ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Of particular concern with plasma-based stripping and cleaning processes is ion-induced and UV-induced damage [181,182]. Ion-induced damage occurs when ions from the plasma bombard the films causing either electrical damage or physical damage. In charging damage, ions transfer charge to the surface, which if severe, af...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
During the cleaning process, Si or SiO2 may be etched, which leads to microscopic surface roughening and material loss. Loss of critical material around sensitive features may lead to current leakage. Diffusion of H into the bulk of the crystal is also an issue with H2-based plasma processing because of bulk-structural...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Traditionally, separation of the plasma generation region from the substrate has been sufficient to minimize high-energy ions that may travel to the substrate. However, to augment this recombination and absorption, Faraday cages and UV-blocking windows have been incorporated into the design of plasma systems. In partic...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
With the incorporation of RF bias, the plasma has direct contact to the substrate; the substrate is surrounded by the plasma sheath similar to plasma damage in an etch chamber. Damage from plasma stripping and cleaning is frequently observed. RF bias can generate charged particles in the plasma above the wafer, resulti...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Plasma-related damage is observed at various steps of the device manufacturing process. Plasma-induced substrate damage occurs during highdose implant resist strip processes. Chan et al. [189] observed device damage at the HDIS step and controlled this damage by optimization of the source (ICP) and bias (RF) power, whi...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## Acknowledgments We acknowledge helpful discussions with Alex Kabansky. Shawming Ma of Mattson Technology is thanked for his contribution to the third edition. ## References [1] Semiconductor Industry Association, The International Technology Roadmap for Semiconductors, 2015. [2] J. Langan, P. Maroulis, R. Ridgew...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Technol. A6 (1988) 950. [21] J. Len, K.F. Jensen, J. Vac. Sci. Technol. A9 (1991) 2948. [22] M.R. Baklanov, S. Vanhaelemeersch, H. Bender, K. Maex, J. Vac. Sci. Technol. B17 (1999) 372. [23] S. Fujimura, K. Shinagawa, M. Nakamura, H. Yano, Jpn. J. Appl. Phys. 29 (1990) 2165. [24] S. Fujimura, K. Shinagawa, M.T. Suz...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[33] S. Savas, J. Zajac, R. Guerra, W. Helle, US Patent 6,805,139, 2004. [34] C. Jehoul, K. Van Baekel, W. Boullart, H. Struyf, S. Vanhaelemeersch, US Patent 6,352,936, 2002. [35] L. Diao, S. Xu, ECS Trans. 18 (1) (2009) 663. [36] V. Vaniapura, S. Ma, B. Elliston, H.-A. Phan-Vu, D. Liou, K. Kang, A Novel Post High Dos...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[45] S.G. Robello, W. Graff, V. Krishna, J. Merriam, P. Keswick, Solid State Technol. 46 (12) (December 2003) 38. [46] C.W. Lee, in: J. Ruzyllo, R.E. Novak (Eds.), Fourth International Symposium on Cleaning Technology in Semiconductor Device Manufacturing, vol. 95-20, The Electrochemical Society, Pennington, NJ, 1995,...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
146 (6) (1999) 2318. [58] J.P. Simko, G.S. Oehrlein, T.M. Mayer, J. Electrochem. Soc. 138 (1) (1991) 277. [59] A.E. Braun, Semicond. Int. 28 (5) (May 2005) 41. [60] M.-S. Kuo, X. Hua, G.S. Oehrlein, A. Ali, P. Jiang, P. Lazzeri, M. Anderle, J. Vac. Sci. Technol. B28 (2010) 284. [61] J. Bao, H. Shi, J. Liu, H. Huan...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[68] J.A. Shields, L. You, M.R. Rakhshandehroo, US Patent 6,794,298, September 21, 2004. [69] S. Lamy, O. Louveau, G. Fanget, M. Fayolle, N. Rochat, D. Louis, L. Broussous, in: IEEE International Interconnect Technology Conference (IITC), 2002, p. 30. [70] S. Lin, C. Jin, L. Lui, M. Tsai, M. Daniels, A. Gonzalez, J.T...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Solid State Sci. Technol. 4 (2015) N5054. [79] K.J. Kanarik, T. Lill, E.A. Hudson, S. Sriraman, S. Tan, J. Marks, J.V. Vahedi, R.A. Gottscho, J. Vac. Sci. Technol. A 33 (2015) 020802-1. [80] G.S. Oehrlein, D. Metzler, C. Li, ECS J. Solid State Sci. Technol. 4 (2015) N5041. [81] E. Vogli, D. Metzler, G.S. Oehrlein, A...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[93] J. Ramm, H. von Kaenel, Future Fab. Int. (November 7, 2003) 15. [94] K.-H. Hwang, E. Yoon, J. Electrochem. Soc. 144 (1) (1997) 335. [95] B. Anthony, L. Breaux, T. Hsu, S. Banerjee, A. Tasch, J. Vac. Sci. Technol. B7 (1989) 621. [96] T.-R. Yew, R. Reif, J. Appl. Phys. 68 (1990) 4681. [97] T.-R. Yew, R. Reif, J. App...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[108] T.P. Schneider, J. Cho, D.A. Aldrich, Y.L. Chen, D. Maher, R.J. Nemanich, in: J. Ruzyllo, R.E. Novak (Eds.), Second International Symposium of Cleaning Technology in Semiconductor Device Manufacturing, vol. 92-12, The Electrochemical Society, Pennington, NJ, 1992, p. 122. [109] J. Abrefah, D.R. Olander, Surf. Sc...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[120] T. Taguwa, K. Urabe, M. Sekine, Y. Yamada, T. Kikkawa, IEEE Trans. Electron. Dev. 44 (4) (1997) 588. [121] S. Subrahmanyan, L.-Y. Chen, R.C. Mosely, US Patent 6,905,965, June 14, 2005. [122] Z. Falkenstein, M. Hakovirta, M. Nastasi, Thin Solid Films 381 (1e2) (2001) 84. [123] E.T. Ogawa, J.W. McPherson, J.A. R...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[133] A.D. Johnson, W.R. Entley, P.J. Maroulis, Solid State Technology, December 2000, p. 103. [134] J. Cox, S. Koenigseder, T. Decker, Micro (March 2001) 89. [135] J. Hackenberg, B. Holbrook, T. Ingwersen, in: G.S. Mathad, G.C. Schwartz, D.W. Hess (Eds.), Seventh Symposium on Plasma Processing, vol. 88-22, The Electr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[147] M. Cantagrel, M. Marchal, J. Mater. Sci. 8 (12) (1973) 1711. [148] S. Fujimura, H. Yano, J. Electrochem. Soc. 135 (1988) 1195. [149] B.A. Thedjoisworo, D. Cheung, D. Zamani, J. Vac. Sci. Technol. A30 (3) (2012) 031303-1. [150] A.R. Reinberg, US Patent 3,757,733, September 11, 1973. [151] A.R. Reinberg, R.K. Rao...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[168] M. Read, W. Schwarz, D. Oakes, in: IEEE 31st International Conference on Plasma Science, 2004, p. 307. [169] J.Y. Jeong, J. Park, I. Henins, S.E. Babayan, V.J. Tu, G.S. Selwyn, G. Ding, R.F. Hicks, J. Phys. Chem. A204 (2000) 8027. [170] O. Auciello, D.L. Flamm, Plasma Diagnostics: Discharge Parameters and Chemi...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[181] S.A. Bell, D.W. Hess, J. Electrochem. Soc. 139 (1992) 2904. [182] Y. Kawamoto, in: Proceedings of the Seventh Symposium on Dry Processing, vol. 5, 1985, p. 132. [183] S.J. Pearson, J.W. Corbett, T.S. Shi, Appl. Phys. A43 (1987) 153. [184] S. Savas, in: IEEE Plasma- and Process-induced Damage, 1st International S...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
[192] T. Mizutani, S. Nishimatsu, J. Vac. Sci. Technol. A6 (1988) 1417. [193] K. Panda, D. Economou, J. Vac. Sci. Technol. A19 (2002) 1566. [194] S. Samukawa, ECS J. Solid State Sci. Technol. 4 (2015) N5089. This page intentionally left blank # Cryogenic Aerosols And Supercritical Fluid Cleaning And Surface Condition...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
8.3.4 Applications Using ![476_image_5.png](476_image_5.png) Supercritical Fluid Cleaning 480 8.3.4.1 Photoresist and Polymer Removal 480 ![476_image_3.png](476_image_3.png) Removal 485 8.3.6 Supercritical Fluid Metal ![476_image_0.png](476_image_0.png) ![476_image_1.png](476_image_1.png) ![476_image_2.png](476_...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress