text stringlengths 1 2k | question stringclasses 1
value | answer stringclasses 1
value | label stringclasses 1
value | origin stringclasses 18
values |
|---|---|---|---|---|
Over the years many cleaning technologies, such as aqueous solution, solvent, plasma, vapor phase, laser, dense phase liquid, UV/O3 (ultraviolet/ ozone), cryogenic aerosol, and supercritical carbon dioxide (CO2), have been used and some are discussed in other chapters of this Handbook. In this chapter, two cleaning met... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The removal of submicron particles in front-end-of-line (FEOL) cleaning is conventionally performed with aqueous methods using standard clean 1 (SC-1)
consisting of NH4OH/H2O2/H2O at a typical ratio of 1:1:5, with the addition of megasonic energy or nitrogen atomization. Chapters 1 and 4 provide in-depth discussions of... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The evolution of device manufacturing technology has resulted in the need to remove particles and other contaminants with minimum loss of SiO2 and polysilicon (polySi) films [1]. Specifically, the ITRS FEOL roadmap states that less than 0.4-A˚ of SiO2 and polySi may be lost at the 45-nm technology node and below. Furth... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The IC manufacturing industry is continuously improving existing cleaning methods, and simultaneously, examining new cleaning technologies to address the surface conditioning needs. Two such cleaning methods, cryogenic aerosol and SCCO2, will be described in this chapter. Section 8.2 will focus on cryogenic aerosols an... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
In BEOL, the post-CMP cleaning requires removal of slurry particles from hydrophobic films such as low-k films or CMP hardmask materials [15,16]. The predominantly physical mechanism of particle removal using cryogenic cleaning lends itself equally effective to films of low or high surface energies.
Another potential ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
A cryogen (noun) by definition is a liquid, such as liquid N2, that boils at a temperature below 110K (160C). Cryogenic (adjective) refers in general to low-temperature processes or phenomena. An aerosol is a suspension of solid particles or liquid droplets in a gas. Thus the phrase "cryogenic aerosol" implies a very c... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
| [24] | Normal Boiling | Normal Boiling |
|----------------------|------------------|------------------|
| Gas | Point (K) | Point (C) |
| Air | 78.7 | 194.5 |
| Nitrogen (N2) | 77.4 | 195.8 ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.2.2 Thermodynamic Properties Of Gases Suitable For Cryogenic Aerosol Formation
To understand the thermodynamic principles governing aerosol formation of cryogenic fluids, an understanding of the triple point is important [25]. At the triple point condition, all three states of matter (solid, liquid, and gas) coex... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
| TABLE 8.2-2 | Pressure and Temperature Values of | |
|---------------------------------------------------------------------------|--------------------------------------|----|
| Cryogenic Gases at Triple Point [26] Triple Point ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Compiled by S. Banerjee and L.B. Rothman from data published by the
Gulf Publishing Company.
The operating conditions (pressure and temperature) of equipment employing cryogenic aerosols are determined by the triple point. In general, the operating condition is lower than the pressure and temperature of the triple po... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
| as Cryogenic Fluids. Updated January 2017 Gas Price Per Ton (US$) Nitrogen (N2) 160 Carbon dioxide 110 Hydrogen (H2) 7700 Neon (Ne) 300,000 Argon (Ar) 1000 Krypton (Kr) 85,000 Xenon (Xe) 1,850,000 |
|--------------------------------------------------------------------------------------------------------------------... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The aerosol in a CO2 cleaning system is formed by first extracting the fluid from the cylinders, which is then expanded through an orifice of a specially designed nozzle [27,28]. The cleaning chamber is at atmospheric pressure.
Thus the fluid undergoes an adiabatic expansion in the nozzle. During this expansion proces... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

Liquid CO2 is in equilibrium with its vapor phase at 850 psia in Fig. 8.2-3, on the border of the liquid and liquidevapor regions. Thus starting from liquid phase at 850 psia, as CO2 expands through the nozzle in an adiabatic and isoenthalpic manner, some of the liquid initially con... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.2.4 Thermodynamics Of Ar/N2 Cryogenic Aerosol System
The cryogenic aerosol formed from Ar and/or N2 gas is similar to the phase change that occurs with CO2 cryogenic aerosol, outlined in Section 8.2-3. The gaseous Ar or Ar/N2 is first extracted from the cylinder at 110 psia and at an ambient temperature of about ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

Extension of cryogenic aerosols to remove nanometer-sized defects without damage is currently under study [22,23]. Modification to the precooling of the Ar or Ar/N2 mixtures have resulted in an aerosol that greatly improves particle removal efficiency (PRE) for particles smaller tha... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

surface. A purge gas, such as N2, flowing parallel to the wafer surface, is used as a curtain to keep the particle from redepositing onto the wafer surface from which it is removed.
The flow of purge gas and the gaseous component of the aerosol stream over the Si wafer surface crea... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Fig. 8.2-6 shows a calculation of the velocity of cryogenic particles crossing a 50-mm-thick boundary layer at an angle of 45degrees to the substrate. The figure indicates that particles larger than 2 mm can cross the boundary layer with greater than 90% of their initial velocity [14,18,27].
In general, particle remov... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

humidity is less than 35C dew point) the capillary and Coulombic image forces do not contribute significantly to the force of adhesion and are neglected.
Thus van der Waals is the dominant particleesubstrate force of adhesion for this aerosol cleaning method for submicrometer parti... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The normal collision force FCN is a sine function of the impact angle:
FCN ¼ FC sin q (8.2-4)

$$(8.2{\bf\cdot}5)$$
$$\cos\,\theta$$
whereas the tangential collision force is a cosine function:
FCT ¼ FC cos q (8.2-5)
The angle of impact plays an important role in determining the re... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
It is therefore important to have a smaller cryogenic aerosol size distribution for effective removal of submicrometer particles below 0.045 mm
(45 nm). These smaller cryogenic aerosols have sufficient force for removal of the submicrometer particles but without the damaging aspect of cryogenic cleaning [20e23]. The re... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.2.7 Examples Of Cryogenic Cleaning Applications In Microelectronic Manufacturing
Section 8.1-2 described the various applications of cryogenic aerosol cleaning for IC manufacturing processes. In this section, some specific examples and results of those applications are presented.
Researchers compared the N2 cryo... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||


of size 10 and 0.2 mm. The X-ray photoelectron spectroscopy (XPS) analysis, shown in Fig. 8.2-11B, indicates that both particles contain copper
(Cu). The Ar/N2 cryogenic aerosol cleaning process successfully removed both particles.
Fig. 8.2-12 s... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Damage-free performance is enhanced with the modified cryogenic aerosol; for example, polySi lines with a 22 nm critical dimension and 200 nm height were processed without damage by the modified cryogenic aerosol. The current cryogenic aerosol, although able to process larger critical dimension and lower height feature... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.3 Introduction To Supercritical And Densified Fluid Cleaning
The discovery of SCF dates back to 1879 when Hanney and Hogarth reported
[42] on the ability of a supercritical fluid to dissolve lowevapor pressure solid materials. They found that gases could be good solvents under supercritical conditions and that th... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
In the mid-1990s an interest in cleaning semiconductor devices with SCF
began. This was partially driven by a desire to reduce H2O and chemical consumption for cleaning semiconductor wafers. In addition to these environmental concerns, there were technical challenges for cleaning the increasingly complex semiconductor ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
An outgrowth of this was cooperative research and development work between Los Alamos National Laboratory (LANL) and industrial partners, which culminated in the development of the SCORR (SCCO2 for resist removal)
system [52]. Research and development work at IBM [53] and the formation of two supercritical fluid equipm... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.3.1 Definition Of Supercritical Fluids
SCF are compounds that exist above their critical temperature and critical pressure. SCF are considered a fourth state of matter where the material is neither a liquid nor a gas, but has the properties of both. In the supercritical state, the fluid has the diffusivity of a g... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
| TABLE 8.3-4 | Critical Parameters for a Range of Gases and Liquids [56] Critical Pressure Critical Density (g/cm3 ) (Psia) Critical Temperature (C) | | |
|---------------------------------------------------------------------... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Compiled by S. Banerjee and L.B. Rothman from Data Obtained from the National Institute of Standards and Technology.
and pressures. Carbon dioxide stands out because the supercritical point is at 31C and 1070 psia (11.5 atm), a temperature that is easy to achieve, although the pressure is higher than other possible SC... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||


that of liquid CO2 (rliquid ¼ 0.86 g/cm3 at 10C); consequently, mass transport of a reactant is quite rapid, even for low concentrations. Furthermore, the solubility of many cosolvents into CO2 is dependent on the density of the CO2.
Because of ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
3. The cofluid reservoir and pump add cosolvents or other additives to the CO2.
4. A heater is used to raise the temperature above the critical temperature and to the desired working temperature.
5. The processing vessel is provided where the wafer is placed and the process occurs.


The additional requirement is that there be sufficient fluid flow to remove the debonded photoresist. If the fluid flow is insufficient, the debonded photoresist remains on the wafer surface. The similarity exists with respect to the thinning of ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

exerted on the polymer often results in a temporarily enhanced polymer swelling effect. Before the polymer/polymer interactions can be reestablished, stress cracks, bubbles, or complete debonding of the polymer film can occur as the CO2 rapidly desorbs. For the photoresist to be com... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Levitin et al. [62] investigated the reactions between tetramethylammonium hydroxide and CO2 for removing photoresist and postetch residues.
Studies demonstrated that it is the bicarbonate salt acting as the active ingredient for cleaning. The use of tetramethylammonium bicarbonate as an effective additive to the SCCO... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Experimental results indicated that 80% of poststripping residues is removed with pure H2O-in-CO2 microemulsions; however, for complete 100%
removal of residues the addition of active chemistry is required [63]. SEM and transmission electron microscopy (TEM) images are shown in Fig. 8.3-24.
 are extremely sensitive to absorbed H2O (k ¼ 78), prevention and... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Owing to their polar nature, these hydroxyl (eOH) groups will impact the dielectric constant of the ILD films directly by increasing the film orientational polarization, and indirectly through the absorption of moisture. As stated

previously, pure SCCO2, despite limited solubility,... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||


small pore sizes commensurate with current scaling needs. CVD deposition also allows graded densities and controlled fraction of hydrophobic groups.
The reason for the preference of silylation reaction with isolated or vicinal silanols of the po... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Although the reaction moiety preferences associated with SCCO2 silylation reaction are not well understood, exposures to silylating agents increase the film contact angle (i.e., hydrophobicity) at relatively low concentrations, 1 vol
% (volume percent), and short reaction times, 1e2 min [78]. As discussed previously, t... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Reaction of vicinal species to form bridged O-species occurs during bakes of 400C. Plasma-stripped porous low-k samples that are baked before silylation exhibit lower contact angles, suggesting that the vicinal species are no longer available for silylation and fewer trimethylsilyl groups are produced.
Pressure and te... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Dynamic secondary ion mass spectroscopy results suggest the depth of the silylation repair is limited [77]. Increased pressure and temperature of the supercritical medium increases the penetration of HMDS into the porous film; however, SIMS results do not show a significant difference between the C-depth profiles of th... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
SCCO2 repair of the plasma-damaged low-k also prevents film loss during subsequent wet etching steps [92]. The plasma-induced loss of hydrophobic methyl functionalities leaves the-MSQ (methylsilsesquioxane) vulnerable to aqueous attack; in the case of H2/N2 plasma-stripped MSQ as much as 1000 A˚
of the MSQ film may be ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
For the largest pitch case, the capacitance is reduced by only 7%. Because the plasma-damaged region between the metal lines is approximately constant, the proportion of the capacitance due to the damage is much larger for the smaller pitch sample, as shown in Fig. 8.3-34. Consequently, the repair of the dielectric con... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.3.6.2 Etching Of Silica
SCCO2 with F-based additives is shown to effectively etch silica-based films.
Dilute solutions of 0.05 vol% HF/ethanol in SCCO2 are capable of removing a 300-nm blanket porous low-k film in less than 60 s [98]. Owing to limited pore penetration, this rate is slowed if the etchant is dilut... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 8.3.7 Pore Sealing
Metal intrusion into porous low-k films during deposition limits device performance and reliability. Metal species penetration into pores can increase the effective dielectric constant (keff) and current leakage, and lower the breakdown voltage. The addition of SiN or SiCN barrier layers to inhib... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

high-resolution TEM results showed that ruthenium (Ru) can be prevented from penetrating into a plasma-damaged MSQ film after exposure to HMDS
[106]. Monoalkylchlorosilanes show promising results with respect to increasing the contact angles, thus increasing the hydrophobicity, as a... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Several groups developed photoresists that are deposited, and later stripped in SCCO2 [114e117]. SCF are employed to develop resists using CO2compatible salts [118].
## 8.4 Summary Of Supercritical Fluids
SCF are a potential processing technology for the semiconductor industry. In this chapter, techniques are outline... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
In addition to cleaning, there are several areas where supercritical fluid technology shows great promise. Device-quality metal and dielectric films have been successfully deposited using SCF. Porogens for templated low-k films are efficiently removed using SCCO2. Some efforts indicate that supercritical processes can ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## Acknowledgments
The authors would like to acknowledge the previous contribution to the second edition by Souvik Banerjee and Laura B. Rothman Mauer, plus the support of Phil Matz, Texas Instruments, the National Science Foundation DMR No. 0316916, and Sematech.
## References
[1] The International Technology Roadm... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[13] R.P. Donovan, Particle Control for Semiconductor Manufacturing, Marcel Dekker, New York, 1990.
[14] S. Banerjee, A. Via, H. Chung, Semicond. Int. Web Article (February 2003).
[15] K.H. Block, H.L. Rayle, Semicond. Int. 25 (6) (June 2002) 115. [16] S. Banerjee, A. Via, S. Joshi, J. Eklund, in: J. Ruzyllo, T. Hatt... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[25] Discussions with Dr. Shuen-Cheng Huang of BOC Group, Murray Hill, New Jersey, 1967. [26] http://www.chemicalogic.com/Documents/co2_phase_diagram.xls and NIST Webbook
(http://webbook.nist.gov/cgi/cbook.cgi?Name=carbonþdioxide&Units=SI&cTG=on&cTC=
on&cTP=on\#Thermo-Phase).
[27] S. Banerjee, A. Campbell, J. Adhesion... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[39] J.W. Butterbaugh, S. Loper, G.P. Thomes, MICRO 17 (6) (1999) 33.
[40] T.J. Wagener, K. Kawaguchi, IEEE/SEMI Advanced Semiconductor Manufacturing Conference and Workshop, 2004, p. 467.
[42] J.B. Hannay, J. Hogarth, Proc. Roy. Soc. Lond. 29 (1879) 324.
[43] U.B. Kompella, K. Koushik, Crit. Rev. Ther. Drug Carr. S... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[55] A.H. Romang, J.J. Watkins, Chem. Rev. 110 (2010) 459. [56] National Institute of Standards and Technology (KIST) Chemistry Webbook, http://
webbook.nist.gov/chemistry/fluid.
[57] J. McClain, C. Case, Micro 22 (1) (January/February, 2004) 33.
[58] L.B. Rothman, NSF/SRC Engineering Research Center for Environmenta... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[66] M.A. Biberger, P. Schilling, Semicond. Fabtech 12 (2002) 239.
[67] L.B. Rothman, R.J. Robey, M.K. Ali, D.J. Mount, IEEE/SEMI Advanced Semiconductor Manufacturing Conference (ASMC), 2002, p. 372.
[68] S.P. Sawan, T.T. Shieh, J.H. Su, G. Manivannan, in: J. McHardy, S.P. Sawan (Eds.), Supercritical Fluid Cleaning: ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[79] B. Xie, A.J. Muscat, Microelectron. Eng. 76 (2004) 53. [80] A. Danel, C. Millet, V. Perrut, V. Daviot, V. Jousseaume, T. Louveau, D. Louis, IEEE
International Interconnect Technical Conference (IITC), 2003, p. 248.
[81] B. Lahlouh, J.A. Lubguban, G. Sivaraman, R. Gale, S. Gangopadhyay, Electrochem. Solid State Le... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[90] E. Vinogradova, C.E. Smith, D.W. Mueller, R.F. Reidy, Electrochem. Solid State Lett. 11
(2008) H255.
[91] E. Vinogradova, E. Osei-Yiadom, C.E. Smith, D.W. Mueller, R.F. Reidy, Microelectron.
Eng. 86 (2009) 176.
[92] B.P. Gorman, R.A. Orozco-Teran, Z. Zhang, P.D. Matz, D.W. Mueller, R.F. Reidy, J. Vac.
Sci. Tec... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[103] C. Jezewski, W.A. Lanford, C.J. Wiegand, J.J. Senkevich, T.-M. Lu, Semicond. Int. 27 (5)
(2004) 56.
[104] T. Abell, K. Maez, Microelectron. Eng. 76 (2004) 16.
[105] E. Vyhmeister, L. Reyes-Bozo, R. Rodrı´guez-Maecker, A. Muscat, D. Suleiman, L.A. Este´vez, Chem. Eng. Commun. 203 (2016) 880.
[106] B.P. Gorman, ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[115] E.N. Hoggan, K. Wang, D. Flowers, J.M. DeSimone, R.G. Carbonell, IEEE Trans. Semicond. Manuf. 17 (2004) 510.
[116] G.L. Weibel, C.K. Ober, Microelectron. Eng. 65 (2002) 145. [117] V.Q. Pham, R.J. Ferris, A. Hamad, C.K. Ober, Chem. Mater. 15 (2003) 4893.
[118] J.P. DeYoung, M.I. Wagner, C. Harbinson, M. Miles, A... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
[118] J.P. DeYoung, M.I. Wagner, C. Harbinson, M. Miles, A.E. Zweber, R.G. Carbonell, Advances in Resist Materials and Processing Technology XXIII, SPIE, vol. 6153, 2006, p. 615346.
Section IV
Analytical and Control Aspects This page intentionally left blank
# Surface Chemical Composition And Morphology
Sara M. Rupi... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
| 9.5 | Stability and Reactivity of Hydrogen-Terminated Silicon Surfaces in Solvents | 565 | | | |
|-----------------|--------------------------------------------------------------------------------|-------|-------|------------------... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 9.1 Overview Of Surface Composition And Morphology
The chemical state in which a surface is left subsequent to a cleaning process is as important as the cleaning process itself. A surface that becomes recontaminated before the next processing step will not be useful. The best cleaning techniques are therefore the o... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The chemical composition of the Si surface subsequent to a clean is fundamental to its passivation. The chemically grown oxides exhibit a more complex chemical composition than the high-quality stoichiometric SiO2 that is grown thermally. Thermal oxides have been studied extensively because of their application as gate... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The microstructural state of the surface has been shown to affect subsequent device properties [3e6]. Surface roughness can cause degradation of the breakdown field strengths of thin gate oxides [4e7], leading to decreased channel mobility [3e6]. Both hydrophilic and hydrophobic surface cleaning processes can affect th... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
As early as the 1950s, Atalla, Tannenbaum, and Scheibner [8] recognized the significance of oxide passivation of Si semiconductor devices. Their discovery of the unique passivation properties of thermally grown oxides, which led to remarkable improvements in device performance, is a cornerstone of modern Si technology.... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Although the chemical perfection of the Si/SiO2 interface is well established, the molecular structure is less well understood. It is clear that there is a transition region between the bulk stoichiometric amorphous SiO2 and the crystalline Si substrate of 3e7 A˚ , where suboxides are observed by X-ray photoelectron sp... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Chemically grown oxides are produced by various cleaning techniques that are based on the use of acidic and/or basic H2O2 aqueous solutions. The most widely used system is discussed in-depth in Chapters 1 and 4, the RCA
Standard Clean developed by Kern and Puotinen [13]; a sequential two-step cleaning process where waf... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 9.2.2 Chemical Composition Of Oxidized Surfaces
The properties of chemically grown oxides produced by the various integrated circuit (IC) cleaning techniques are quite similar and have been addressed by Deal et al. [14]. These techniques are covered in Chapter 4 in detail; they include SPM, SC-1 (standard clean 1),... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Chemical oxidation involves species other than Si and O. Aqueous solutions are predominantly composed of H2O and are, therefore, sources of H2O,

OH, and H. Thus, these chemical species are incorporated into the oxide layer to some extent. There is extensive literature on the infrar... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Hydrogen bonding is common to all aqueous solutions and is intimately related to the heat of solvation and to the hydrophilic nature of oxide-covered Si surfaces. Hydrogen-bonded OeH is observed on all chemically grown oxides. An example of an IR absorption spectrum of such a surface is shown in Fig. 9.2-2, where an H-... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

lowest amount of OH on the surface. SC-1 solutions, on the other hand,
 produce larger quantities of OH units on the surface and within the films. It appears that the OH concentration is related to the degree in which the cleaning solutions produc... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
 produce larger quantities of OH units on the surface and within the films. It appears that the OH concentration is related to the degree in which the cleaning solutions produce SiO2. More OH-terminated groups are formed when the oxide formation is less complete and vice versa.
It is... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 9.2.3 Structures And Morphology Of Oxidized Surfaces
The work of Hahn and Henzler [26], Heyns et al. [7], and Ohmi et al. [5] were some of the first to correlate electronic device properties with surface structural properties. Although it is intuitively obvious that surface roughness must be detrimental to semicond... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Near atomic perfection is achieved through surface CMP. Commercial wafers exhibit a typical surface roughness on the order of 2 A˚ RMS (root mean square) and surface finishes produced in the laboratory have approached 1-A˚
RMS [30]. A scanning tunneling microscope (STM) image of such a surface is shown in Fig. 9.2-4 [3... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
As-received Czochralski Si and epitaxial Si substrates both exhibit a surface roughness of w2-A˚ RMS.
The consensus is that the acidic peroxide cleaning processes (SPM or SC-2) do not cause a substantial increase in the microscopic roughness of as-received wafers. The SC-1 cleaning process (typically 1:1:5 NH4OH:-
H2O... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The mechanism leading to the roughening in the basic peroxide solution is not completely understood but is related to the slow but finite Si etching rate in the SC-1 solution (w8 A˚ /min at full strength at 80C) [6]. The acidic peroxide solutions, on the other hand, do not etch and hence do not roughen.
![534_image_0.... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The microscopic mechanism by which the etching roughens the surface also has been investigated. It should be mentioned that etching alone does not necessarily mean the surface roughness will increase. It is nonuniform etching or preferential etching around a defect or contaminant, which is the true culprit. An early ex... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Although the RCA clean was developed over 40 years ago, it has functioned extremely well and is still the dominant clean used before gate oxidation. As gate oxides move into the sub-100 A˚ regime, there has been renewed interest in how trace metal contamination in the pregate cleaning processes affects gate oxide prope... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Another common contaminant on these oxide-covered surfaces is carbon.
Carbon is most likely incorporated in or on these surfaces in the form of hydrocarbons and can come from the chemicals, the H2O used to rinse the wafers, or from the air in the laboratory environment because of material outgassing [42,43]. Trace hyd... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Some contaminants, such as S and Cl, can originate directly from the solution used during the chemical oxidation. Sulfur and chlorine have been observed from the SPM and SC-2 cleaning solutions, respectively (see Chapters 2 and 4). Fluorine, on the other hand, has been observed when the chemical oxidation is preceded b... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Although several early reports of H-termination subsequent to HF etching

of Si surfaces emerged in the time period between 1965 and 1975 [55,56], it was not until 1984 that Ubara, Imura, and Hiraki [57] showed that the removal of SiO2 in HF solutions results in the formation of SiH... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Despite these early works, which clearly pointed to hydride formation upon HF solution etching, it was still widely believed that F was in fact the passivating agent. Raider et al. [61] attributed the hydrophobic nature of HF-etched surfaces to the presence of SieF bonds or adsorbed HF. Licciardello et al.
[62] indica... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The year 1986 was perhaps the turning point in the H- versus F-termination debate. Yablonovitch et al. [18] observed that the F concentration, as measured by XPS, was highly variable and could not be the correct explanation for the remarkable surface passivation achieved subsequent to HF etching. Using IR
spectroscopy,... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

confirms the formation of silicon hydrides upon HF etching and suggests that F
is a contaminant that can be removed by rinsing in H2O.
Both the surface-recombination velocity measurements of Yablonovitch et al. [18] and the extensive XPS and EELS studies of Grundner et al. [68e70]
... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Although no detectable absorption bands are observed in the OeH stretch
(3600 cm1) and CHx stretch (2800 cm1) regions, the sensitivity of these IR
absorption measurements places an upper limit of 10% of an ML for these species.
Fenner et al. [74] used XPS and AES, both more sensitive techniques, for the detection of C... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The main conclusion of the above studies is that H acts as the passivating agent and is the direct result of HF etching. The concentration of contaminants, such as C, O, and F, depends on the details of the processing, in particular, the rinsing procedure after the last etching step directly affects the concentrations ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Thus, HF and its associated forms need be considered in the dissolution mechanism. As an illustration only of the earlier thinking in the field, the attack of SieO bonds by HF molecules is considered; this would occur by the insertion of HF between the SieO atoms. This reaction is depicted schematically in Fig. 9.3-12A... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Ubara et al. [57] were the first to propose a reaction mechanism to get around this dilemma. They recognized that the SieF bond must be highly polar because of the large electronegativity difference between the atoms.
They suggested that the SieF bond causes bond polarization of the SieSi back-bond allowing HF attack ... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The preceding arguments give us a basic understanding of HF etching. As mentioned before in reality, however, the situation is much more complex, including HF, H2F2, HF2
, F, H3Oþ, OH, and sometimes NH4F species together in the solution and in chemical equilibrium with one another. Additionally, there exist steric cons... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
HF2 can be thought of as a more highly solvated form of HF with a weaker bond strength that explains the lower activation energy for SiO2 dissolution
(0.31 eV) and the increased rate of dissolution (factor of 4e5). The role of steric hindrance at the surface is also important. In general terms, confidence should be pla... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 9.3.3 Structure And Morphology Of Hydrogen-Terminated Surfaces
This section starts with the effects of aqueous HF (concentrated and dilute HF solutions) on the surface morphology of Si (100) and Si (111) and then the etching of Si (111) and Si (100) in BHF solutions is separately examined. BHF
is composed of variou... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
## 9.3.3.1 Si (100) And Si (111) Etched In Aqueous Hf Solutions

The first information available on the morphology of H-terminated Si (100) and Si (111) was the study by Hahn and Henzler [26]. Their goal was to use low-energy electron diffraction (LEED) to investigate the Si/SiO2 in... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
Next, Grundner and Schulz [69,70] used the vibrational frequency information from EELS on HF-treated Si (111) and Si (100) to investigate the nature of the H-termination. By monitoring the SiH2 scissor mode of the dihydride species at 900 cm1, they concluded that Si (100) was dihydride terminated while Si (111) was mon... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The roughness is evident from the complexity of the polarized IR
absorption spectra shown in Fig. 9.3-14 for Si (111), for instance. An ideally terminated Si (111) surface would be characterized by a single monohydride stretch mode polarized normal to the surface (see Fig. 9.3-15) and this is not observed in Fig. 9.3-1... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
With these mode assignments, the structure of these H-terminated surfaces can be obtained. However, the assignment of trihydride (T) has been reconsidered as dihydride structures with strong steric interactions, which also have modes at that frequency.
For Si (111), the spectra in Fig. 9.3-14A are dominated by monohyd... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The main conclusion of these results is that Si etching in dilute HF leads to atomically rough surfaces as seen from the presence of mono-, di-, and possibly trihydrides on both Si (100) and Si (111) surfaces, indicating that the initial Si/SiO2 interface is atomically rough. STM images of Si (111) [84]
show structures... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||

etching of defect structures, with the slowest etching occurring on the (111)
planes, thus making it possible to flatten the (111) surface on an atomic scale [84]. For instance, Fig. 9.3-19 shows the difference between a Si (111) surface etched in dilute HF and buffered (pH w8) HF s... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress | ||
The LEED patterns obtained after careful introduction of the H-terminated silicon sample into UHV show a 1 - 1 pattern with resolution-limited integralorder spots and a background below the detection limit of conventional

LEED systems as shown in Fig. 9.3-17. This unreconstructed a... | text_only | 16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress |
Subsets and Splits
No community queries yet
The top public SQL queries from the community will appear here once available.