254e264, 294e295 application of cleaning principle for, 257e259 challenges, 255e256 chemicals, 273e285 acidic and noneSCe1 alkaline solutions for FEOL post-CMP cleaning, 276e278 aluminum metal gate post-CMP cleaning solutions, 279e280 ammonium hydroxide and neutral solutions for tungsten post-CMP cleaning, 278e279 copp...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Pourbaix diagram(s), 106e107, 107f, 258e259 of AleH2O system, 279e280, 279f, 586, 586f Power law size distribution, 102e103 PP. See Polypropylene (PP) PRE. See Particle removal efficiency (PRE) Pre-epitaxial deposition cleaning, 356e357, 413e416 Pre-high-k deposition, 416 Pre-thin film measurement, 361e362 Pre-tungsten...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
PTFE. See Polytetrafluoroethylene (PTFE) Purge gas, 467e468 PVA. See Polyvinyl alcohol (PVA) PVA disks. See Polyvinyl acetal disks (PVA disks) PVD. See Physical vapor deposition (PVD) PWP. See Per-wafer-pass measurements (PWP) Pyrex filter, 337e338 PZC. See Point of zero charge (PZC) Q QDR. See Quick dump rinser (QDR) ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Relative humidity, 125 Relative sensitivity factor (RSF), 721e722 Relative standard deviation (RSD), 685 Reliability classification according to, 92 relationship to defectivity, 92e96 defect size distribution, 95 effective area, 95e96 statistical yield models, 93e94 Reliable detection of particles, 696 Remote ECR pla...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
|-------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| evaluation of rinsing performance, 221e223 process, 651 processors, 231e234 dump rinsing, 231e232 effects of rinse tank configuration, 233f overflow rinsing, 232 spin-spray rinsing, 233e234 ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| RMG. See Replacement metal gate (RMG) RMS. See Root mean square (RMS) Rocking scan, 720 Root mean square (RMS), 130, 513e514, 737 Rotagoni, 28 drying module, 293, 293f system, 59 RPD test. See Reproducibility test (RPD test) RPT test. See Repeatability test (RPT test) RSD. See Relative standard deviation (RSD) RSF. S...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
SCORR process. See scCO2 for resist removal process (SCORR process) Scratch-related alumina residue, 279e280, 280f Scratches, 93 SCS. See Scanning collection solution (SCS) SD. See Standard deviation (SD) Secondary ion mass spectroscopy (SIMS), 27e28, 329, 414e415, 720e724 Segregation gettering, 115 Self-annealing, 592...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
etched in aqueous HF solutions, 528e531 etched in buffered HF solutions, 537e545 etching mechanism, 548e549 Si (111) etched in aqueous HF solutions, 528e531 etched in buffered HF solutions, 531e537 surfaces mechanism, 546e548 Si-rich salts, 336 surfaces analytical measurement, 702 Silicon carbide (SiC), 12 Silicon diox...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
(SIMS) Single-wafer brush scrubbers, 26 chemical processors, 230e231 cleaning, 61e62, 194e195, 234 downstream reactors, 430 immersion tank megasonic module, 289, 290f process modules, 622e623 processing, 24e25, 209e210 single-wafer/short-cycle clean, 21, 24e25, 25f SRDs, 286 tool for immersion wet processing, 25 wet pr...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
"Step flow" etching mechanism, 547e548 Stern layer, 163, 202 STG. See Surface tension gradient (STG) STI. See Shallow trench isolation (STI) "Stiction", 359 Stiction-related pattern collapse, 227 STM. See Scanning tunneling microscope (STM) Strained dihydrides, 543e544 Stripping process, 381e382 Subatmospheric gas-phas...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
(SPM), 8, 137, 188, 391e392, 395, 509, 514e515, 625 photoresist stripping, 198e200 Sulfuric acideozone mixture (SOM), 16e17 "Sum peak", 718e719 Supercritical carbon dioxide (scCO2), 56, 60, 458, 460e461, 476, 482, 484, 487, 493e494, 496e497 cleaning, 60 critical density, 478e479 microemulsions, 484e485 region, 464 repa...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
surface conditioning processes, 28e36 equipment for implementing wet-chemical cleaning, 26e27 liquid processes and wafer drying techniques, 14e15 supercritical fluid metal removal, etching, and copper removal, 494 etching of silica, 494e495 technology, 14e36 wafer rinsing, drying, and storing, 27e28 wet-chemical cleani...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
"T-topping", 121 Tafel plots of Cu and Co, 271, 272f TAZ. See 1,2,4-Triazole (TAZ) TCP. See Transformer-coupled plasma (TCP) TDAeMS. See Thermal Desorption Analysis Gas Chromatography Mass Spectrometry (TDAeMS) TDDB. See Time-dependent dielectric breakdown (TDDB) TDMAT. See Tetrakis-dimethylamido titanium (TDMAT) TE. S...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
TMCS. See Trimethylchlorosilane (TMCS) TOC level. See Total organic carbon level (TOC level) TOFeSIMS. See Time-of-flight secondary ion mass spectrometry (TOFeSIMS) Total organic carbon level (TOC level), 220, 220f, 666 Total reflection X-ray fluorescence (TXRF), 329, 704, 707te709t, 715e719, 715f analysis of SiO2 film...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
ULPA filters. See Ultra-low penetration air filters (ULPA filters) ULSI. See Ultra-large-scale integration (ULSI) Ultra-large-scale integration (ULSI), 5 Ultra-low penetration air filters (ULPA filters), 89, 103e104 Ultraclean, 5e6 sample vial, 710e711 Si, 4 Ultrahigh vacuum (UHV), 520 Ultralow k nanoporous dielectrics...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
Uric acid, 596e597 UV. See Ultraviolet (UV) UV/chlorine (UV/Cl2), 31 dry wafer cleaning, 348f mechanisms, 351e352 for metallic contamination removal, 336e347, 349 recovery of cleanliness, 350f surface impurity concentrations, 350f TXRF data, 348f vapor pressure for "high"evapor pressure metals, 351f of metal chlorides,...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
VPD/Atomic Absorption Spectroscopy (VPD/AAS), 706, 707te709t, 714 VPD/ICPeMS. See Vapor phase decomposition-inductively coupled plasma mass spectrometry (VPD/ICPeMS) VPD/TXRF. See Vapor Phase Decomposition Decomposition/Inductively Coupled Plasma Mass Spectroscopy (VPD/TXRF) W Wafer cleaning, 238e239 alternative wet-ch...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
liquid processes and wafer drying technology, 58e59 trends and milestones, 56e57 technology, 14e36 wafer rinsing, drying, and storing, 27e28 wet-chemical cleaning processes, 15e21 Wafer contamination, 88e101. See also Ultratrace impurity analysis of wafer surfaces aspects, 10e14 behavior and impact of contamination AMC...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
detection, 695 particle monitoring on wafer for cleaning tools, 664e668 particle scan maps with particle reattachment, 288, 288f particulate contamination analysis on, 663e664 rinsing, 27e28 scanning process, 710e711 collection efficiency of scanning process, 711e712 storage, 28 surface, 660e661, 712 analysis, 705 basi...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
"Watermarks", 127e128, 225e227, 226f, 261e262 Wavelength, 628e629 emitted by UV sources, 340e342 ranges, 628e629, 630f Weibull distribution, 94 Wet bench batch immersion processing tanks, 622e623 process, 666 Wet cleaning chemical manufacturers, 193
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| formulation, 412 limitations, 307e308 processes, 187, 653 ...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
|-------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
| Wet etching chemistries, 588e589 Wet processing, 620 chemicals, 624e626, 624t, 645 treatments, 606 Wet stations, particle monitoring of, 665e667, 667f Wet wafer cleaning operations, 307 Wet-chemical, 5, 14 alternative wet-chemical cleaning and surface conditioning systems, 21e25 DDC, 24 IMEC Clean, 22e24, 24f Ohmi Cl...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
This page intentionally left blank ## Third Edition Handbook Of # Silicon Wafer Cleaning Technology ## Edited By Karen Reinhardt And Werner Kern Handbook of Silicon Wafer Cleaning Technology, Third Edition provides an in-depth discussion of cleaning, etching, and surface conditioning for semiconductor applications....
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## Key Features - Focuses on cleaning techniques including wet, plasma, and other surface conditioning techniques used to manufacture integrated circuits - Supplied reliable references for cleaning surface conditioning used for manufacturing integrated circuits - Covers processes, equipment and metrology, including th...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
## Note On Previous Editions The first edition of this well-received handbook was published in 1993, edited by Werner Kern, the inventor of the RCA critical cleaning process. Karen Reinhardt joined as co-editor for the second edition and now leads the efforts for this third edition. ![793_image_0.png](793_image_0.png...
text_only
16_handbook-of-silicon-wafer-cleaning-technology-third-edition_compress
# Plasma-Materials Interactions A Series Edited by Orlando Auciello Microelectronics Center of North Carolina and North Carolina State University Research Triangle Park, North ( Daniel L. Flamm A T& Τ Bell Laboratories Murray Hill, New Jersey Advisory Board J. L. Cecchi Department of Chemical Engineering Princeton Un...
text_only
18_plasma-etching-an-introduction_compress
``` ACADEMIC PRESS, INC. 1250 Sixth Avenue, San Diego, CA 92101-4311 United Kingdom Edition published by ACADEMIC PRESS LIMITED 24-28 Oval Road, London NW1 7DX Library of Congress Cataloging-in-Publication Data ``` Plasma etching. (Plasma: materials interactions) Bibliography: p. Includes index. 1. P...
text_only
18_plasma-etching-an-introduction_compress
Most of our students wanted a text or reference book that covered the course material but, unfortunately, nothing appropriate was available. This new Academic Press series, "Plasma-Materials Interactions," became a logical focus for such a project and stimulated this volume. In Plasma Etching: An Introduction experts a...
text_only
18_plasma-etching-an-introduction_compress
Chapter 4 presents a detailed treatment of several of the most important types of diagnostics used in process plasma research and development and in the production of ULSI devices. These include established diagnostics, such as electrostatic probes and emission spectroscopy, as well as the newer ## Xi techniques of ...
text_only
18_plasma-etching-an-introduction_compress
Daniel L. Flamma and G. Kenneth Herbb AT&T Bell Laboratories a *Murray Hill, New Jersey* h*A llentown, Pennsylvania* | I. Introduction | 2 | | |-----------------------------------------------|------|----| | A. Development of Microelectronics | 2 | | | B. Critical ...
text_only
18_plasma-etching-an-introduction_compress
``` Plasma Etching: An Introduction 1 Copyright © 1989 by Academic Press, Inc. All rights of reproduction in any form reserved. ...
text_only
18_plasma-etching-an-introduction_compress
## I. Introduction The rapid development of plasma etching technology was stimulated by its application to the manufacture of microelectronic devices. Since the early 1970s, when plasma etching was first widely adapted to device manufacturing, a new recognition and understanding of plasma chemistry has emerged. Toda...
text_only
18_plasma-etching-an-introduction_compress
The use of Si0 2 masks for controlling silicon doping by impurities was invented by C. J. Forsch and L. Derick in 1955 [6]. Oxide masking evolved as a key step in the manufacture of silicon integrated circuits. An early integrated circuit (1961 design of Fairchild Camera) is shown in Fig. 2. These first circuits typi...
text_only
18_plasma-etching-an-introduction_compress
![9_image_0.png](9_image_0.png) record of rapid innovation in the microelectronic industry is unmatched in history. ## B. Critical Dimension Decrease The cost of a unit memory cell decreases with increasing circuit density. Figure 4 shows that unit memory cost dropped a factor of 33 over the past decade. This dra...
text_only
18_plasma-etching-an-introduction_compress
![11_image_0.png](11_image_0.png) 2.5 μηι, while the minimum feature dimension in leading edge designs dropped from 2.0 μ m to 0.75 μ m. The complexity and functionality of circuit design has grown along with decreasing feature size. This complexity introduced additional masking steps in device production. At the same...
text_only
18_plasma-etching-an-introduction_compress
FEATURE SIZE (TIGHTEST-MICRONS) 2.0 2.0 1.5 1.5 1.0 0.7 ALIGNMENT (TIGHTEST OVERALL FIT-MICRONS) 1.0 1.0 0.7 0.5 0.3 0.2 WAFER SIZE (% 100mm/% 125 mm) 99 97 95 90 80 60 MASKING STEPS (MINIMUM) 5 + 1 5 + 1 6 + 1 6 + 1 6 + 1 6 + 1 MASKING STEPS (MAXIMUM) 10 + 1 10 + 1 11 + 1 11 + 1 12 + 1 12 + 1 DIELECTRIC THIC...
text_only
18_plasma-etching-an-introduction_compress
## C. Process Defect Density To make these advanced designs possible, the fabrication process must provide an improved "zero defect" capability. The key process parameter that measures this capability is the *fatal defect density,* or DQ . With 1980 technology, a DQ of 3 defects per cm2 gave about 70% circuit yield f...
text_only
18_plasma-etching-an-introduction_compress
A pattern is commonly formed by either the *additive or subtractive* method, as illustrated in Fig. 7. In both methods the objective is to produce ![14_image_0.png](14_image_0.png) a patterned thin film on a substrate. In the subtractive process this film is first deposited as a uniform layer by chemical vapor depos...
text_only
18_plasma-etching-an-introduction_compress
``` | PROCESS STEP | | | |------------------------------|-------|-----------| | GROW THIN OXIDE | X | | | DEPOSIT NITRIDE | X | | | CONDITION NITRIDE | X | | | MASK I1DEFINE FIELD | X | ...
text_only
18_plasma-etching-an-introduction_compress
![15_image_0.png](15_image_0.png) soluble (or insoluble) to a developer-solvent. The developer dissolves unwanted areas creating the final mask pattern. The resist pattern now becomes a stencil that will protect the underlying film from attack by the etching process, which is the next step in the pattern transfer op...
text_only
18_plasma-etching-an-introduction_compress
Plasma etching can be applied to steps in both processes. ## E. Isotropic An D Anisotropic Etching Differences in etching mechanisms have an immediate effect on the profiles of features in both "wet " chemical and "dry" plasma chemical etching. Purely chemical etching usually has no preferential direction. This le...
text_only
18_plasma-etching-an-introduction_compress
It is important to add that the formation of vertical walls on etched features does not necessarily mean that etching was ion enhanced. Vertical profiles are formed in isotropic chemical etching during severe undercutting (as noted before), and can also be produced when there is preferential etching along specific cry...
text_only
18_plasma-etching-an-introduction_compress
## F. Th E Transition From Wet To Plasma Etching Plasma etching was explored as a cheaper alternative to wet solvent resist stripping [16] for integrated circuit manufacture in the late 1960s and early 1970s. By the early 1970s, CF 4 / 0 2 plasma etching was widely adopted for patterning silicon nitride passivation of...
text_only
18_plasma-etching-an-introduction_compress
Because of the isotropic undercut, wet etching a 1 μ m thick film through a 1 μ m mask opening at best yields a cross-sectional profile that measures 3 μ m at the top and 1 /xm on the bottom. Thus with increasing circuit density and narrower linewidth requirements, anisotropic etching became necessary to pattern featur...
text_only
18_plasma-etching-an-introduction_compress
Before going into more detail about reactors and the etching process, we will briefly describe some essential basic characteristics of the plasma environment. To the physicist, a plasma is an ionized gas [17] with equal numbers of free positive and negative charges. The free charge is produced by the passage of electri...
text_only
18_plasma-etching-an-introduction_compress
Generating the same reactive species without a plasma would require temperatures in the - 10 3-10 4 o K range that would incinerate organic photoresist and melt many inorganic films. The coexistence of a warm gas and high temperature active species distinguishes the plasma reactor from conventional thermal processing. ...
text_only
18_plasma-etching-an-introduction_compress
``` o- FIGURE 11. Some basic characteristics of plasmas used for microelectronic processing. ![22_image_0.png](22_image_0.png) phase, forming a thin boundary layer or *sheath.* Because electrons are light and have high energy, they diffuse fastest, leaving an excess of positive charge and a plasma potential that is...
text_only
18_plasma-etching-an-introduction_compress
## A. Wha T Basic Mechanisms Cause Etching? Plasma etching can proceed by physical sputtering or chemical reaction and ion-assisted mechanisms. During sputtering, substrate material is removed by purely physical processes; energetic ions crossing the sheath transfer large amounts of energy and momentum to the substrat...
text_only
18_plasma-etching-an-introduction_compress
Chemical and ion/chemical mechanisms differ from sputtering in that the surface material is first converted into high vapor pressure products to facilitate removal. Mass loss is then evaporative, so that etching can be done at higher pressure where any sputtered material is scattered back onto the surface by gas collis...
text_only
18_plasma-etching-an-introduction_compress
It is sensitive to the magnitude of bonding forces and structure of a surface, rather than its chemical nature and quite different materials can sputter at similar rates. In a way this is symptomatic of using ion bombardment with energy far higher than the surface binding energy. In chemical etching, gas phase specie...
text_only
18_plasma-etching-an-introduction_compress
a substrate. However, the process is usually *isotropic* or nondirectional, [18] which is sometimes a disadvantage. With isotropic etching, both vertical and horizontal material removal proceed at the same rate, making it impossible to form the fine lines (less than about 3 microns in the usual ~ 1 μ-thick films). ...
text_only
18_plasma-etching-an-introduction_compress
The second class, *inhibitor* ion-enhanced etching, requires two conceptually different species: etchants and inhibitors. The substrates and etchants in this mechanism would react spontaneously and etch isotropically, if it were not for the inhibitor species. The inhibitors form a very thin film on (vertical) surfaces ...
text_only
18_plasma-etching-an-introduction_compress
## A. Electron Energy In a system in thermal equilibrium, kinetic and internal energy are uniformly distributed among all the species and degrees of freedom. As a result, the energy in any internal or translational state can be expressed in terms of a single parameter, the temperature T. On the other hand, plasmas are...
text_only
18_plasma-etching-an-introduction_compress
When particles collide without dissociating or absorbing energy into internal states (as with two billiard balls), the collision is said to be *elastic.* The energy transferred from higher-kinetic-energy particles to lower-energy particles in these collisions depends on the distance of closest approach, with the avera...
text_only
18_plasma-etching-an-introduction_compress
## B. Types O F Collisions In the last section we introduced elastic collisions in which particles exchange momentum and kinetic energy without affecting their internal states. *Inelastic* collisions are a second broad category of particle-particle interactions. When inelastic collisions take place, the interacting sp...
text_only
18_plasma-etching-an-introduction_compress
Still, even in molecular gases, the average fraction of energy lost per collision is usually low. Figure 16 shows the average fraction of energy lost per collision in He, N 2 and H 2 (including elastic collisions) as a function of the average electron energy. Note, the fractional energy transferred by elastic collisio...
text_only
18_plasma-etching-an-introduction_compress
$$e E\lambda=\kappa(\epsilon_{e}-\epsilon_{g}),$$ eEX = K(ee-eg), (5) and then solve for (ee - eg), $$({\mathfrak{s}})$$ $$\epsilon_{e}-\epsilon_{g}=\frac{e E\lambda}{\kappa}\approx\epsilon_{e}=\frac{E\lambda}{\kappa}\;\mathrm{eV}.$$ $$(\mathbf{6})$$ We see that a small κ means high energy electrons. For typical ...
text_only
18_plasma-etching-an-introduction_compress
$$e\,+\,{\bf O}_{2}\,\rightarrow\,{\bf O}_{2}^{+}+\,2\,e\,,$$ $$(8\mathbf{a})$$ + *le,* (8a) b) atom and radical formation $$e\,+\,\mathrm{O}_{2}\,\rightarrow\,\mathrm{O}\,+\,\mathrm{O},\,\mathrm{and}$$ -> Ο + Ο, and (8b) c) generation of heat and light $$e\,+\,\mathbf{O}_{2}\rightarrow\mathbf{O}_{2}^{\star}\,...
text_only
18_plasma-etching-an-introduction_compress
In the plasma, each formation step balances various loss processes. The equilibrium between formation and loss determines the steady concentrations of species in a discharge. For the charged species in a plasma, these formation and loss processes may be grouped into a few categories as follows. 1. Ionization and Deta...
text_only
18_plasma-etching-an-introduction_compress
$$C^{\star}\,+\,A B\,\to\,C\,+\,A^{\,+}\,+\,B\,+\,e,$$ C* + AB -> C + A + *+ Β + e,* (12b) or $$C^{\star}\,+\,M\to C M^{+}+\,e\,.$$ $$(12\mathrm{c})$$ C* + M -> CM ++ e. (12c) Penning ionization has been found to be significant in mixtures where C is a rare gas with a metastable state excitation energy (e.g., Ne) t...
text_only
18_plasma-etching-an-introduction_compress
in a pure argon discharge only simple electron-ion recombination is possible $$(15)$$ $$(16)$$ $$e+A^{+}\to A.$$ e + A + *^A.* (16) In highly exothermic reactions, reaction channels that form two or more product fragments with comparable mass are generally favored, because they make it easier (there are more configu...
text_only
18_plasma-etching-an-introduction_compress
Kinetic theory 2 4 shows that *random* thermal motion of a gas results in a flux, $$(17)$$ $${\dot{j}}={\bar{n}}{\frac{\bar{v}}{4}}={\frac{\bar{n}}{4}}\,{\sqrt{\frac{8k T}{\pi m_{j}}}}$$ of particles to the wall, where mt is the mass of gas molecules. Since there is an intense electric field *in the sheath,* the cha...
text_only
18_plasma-etching-an-introduction_compress
(17). These phenomena usually force the average wall potential to be negative relative to the higher density plasma in the (more nearly equipotential) glow region. The potential in the glow is termed the plasma potential. Since electrons have an average energy kTe /t, this is, roughly, the magnitude of the floating p...
text_only
18_plasma-etching-an-introduction_compress
![35_image_0.png](35_image_0.png) ![35_image_1.png](35_image_1.png) FIGUR **E 17. An insulating wall placed in a plasma charges to a negative potential because** the random electron flux is larger than the ion flux (upper diagram). But the steady current must finally fall to zero or the negative wall potential would...
text_only
18_plasma-etching-an-introduction_compress
$$(19)$$ ![36_image_0.png](36_image_0.png) highest energy electrons (at the top of the electron energy distribution function) overcome the applied bias and reach the probe. When the potential reaches Vf , there is no net current to the probe. At Vf , electrons are repelled to the point that their current is just equa...
text_only
18_plasma-etching-an-introduction_compress
## 3. Potentials And Dc Bias At The Electrode Sheaths In the last section, it was pointed out that most of the applied potential appears across the plasma sheaths; however, the analyses treated uniform steady fields and voltages in contrast to the RF alternating current generally used for device processing. The high m...
text_only
18_plasma-etching-an-introduction_compress
This asymmetric electrode-plasma current-voltage characteristic approximates a leaky diode in parallel with the sheath capacitance (Fig. 19). In most cases, the RF source, which supplies power, has an unbalanced feed (e.g., one lead is connected to chassis common or ground) and there is a "blocking" capacitor in seri...
text_only
18_plasma-etching-an-introduction_compress
When one of the electrodes is smaller than the other, a larger voltage is developed across the smaller (Cs) sheath capacitance. Again, if the blocking capacitor is large, a simplified circuit analysis suggests the voltage across the smaller electrode sheath modelled in Fig. 19 is given by $$V_{s}\,,_{\rm sheath}=\fra...
text_only
18_plasma-etching-an-introduction_compress
![39_image_0.png](39_image_0.png) The larger RF voltage drop causes intensified ion bombardment at the smaller electrode. There is another minor effect, which is not represented in Figs. 19 and 20. Electrons can cross potentials as large as their average energy, usually a few volts. This energy acts to offset the ...
text_only
18_plasma-etching-an-introduction_compress
19), however, is probably not good enough for estimating the potentials in low frequency discharges where highly non-linear voltage current relationships are involved. These sheath potentials and voltage-current characteristics need further study. ## 4. Effects Of Pressure And Frequency On Sheath Potentials As press...
text_only
18_plasma-etching-an-introduction_compress
Consequently, we see that frequency and pressure are, to an extent, interchangable variables. Either low frequency or low pressure can be used to increase sheath potentials. The important differences are that with low ![41_image_0.png](41_image_0.png) ![41_image_1.png](41_image_1.png) pressure, the concentration of...
text_only
18_plasma-etching-an-introduction_compress
Reactive ion etching (RIE) is another misused phrase. By definition this term should be used for etching by ions that react with and remove substrate material (e.g., "hungry ions"). As we will see, with this meaning any reactive ion etching is rare, unless beam ion sources are used at lower pressure (see Chapter 6). Un...
text_only
18_plasma-etching-an-introduction_compress
| Number | Molecular | Wall | Mean Free | | |-----------------------------------------------------------------|----------------|-----------------------------------|-------------|--------| | Density ...
text_only
18_plasma-etching-an-introduction_compress
| 298 Κ, 1 Ton | | | | | | (M=4, r o=1.09Â) | 3.3 χ 101 6 | 12350 | 1.6 xlO2 1 | 0.014 | | He ...
text_only
18_plasma-etching-an-introduction_compress
dependencies should be noticed. Gas density and molecular flux to a surface are proportional to pressure at constant temperature. The mean free path λ of species is inversely proportional to density, pressure, and collision cross sections (square of the molecular radius sum). Mean free paths and molecular collision dia...
text_only
18_plasma-etching-an-introduction_compress
## G. Sequential Steps In Etching The etching process can be viewed as a series of steps illustrated by the energy-driven ion assisted etching of *undoped* silicon by chlorine: (I) ion and electron formation (which balances loss of charged species and is part of a more complex reaction set) $$e\,+\,\left\{\begin{ar...
text_only
18_plasma-etching-an-introduction_compress
$$(25)$$ $$\left.\begin{array}{l}\mbox{SiCl}_{x(ads)}\rightarrow\mbox{SiCl}_{x(gas)}\,^{+}\\ \end{array}\right.\tag{1}$$ $$(26)$$ For completeness, surface diffusion of adsorbed reactants or reactive intermediates should also be considered since some evidence for such a step has been observed. Chemical etching proceed...
text_only
18_plasma-etching-an-introduction_compress
The evaporation rates of a material *(A)* of molecular weight Ma is proportional to its vapor pressure (30), pa , $$\mu_{A}=\alpha\left[\frac{M_{a}}{2\pi R T}\right]^{-1/2}p_{A}.$$ $$(27)$$ Experiments show the material-dependent efficiency factor a, is usually between 0.1 and 1.0. The vapor pressure pA in turn dep...
text_only
18_plasma-etching-an-introduction_compress
Experiments show that plasma etching of InP at ~ 0.1-1 Torr is rate-limited by InCl 3 sublimation [32]. The etch rate has an activation energy (slope of rate versus 1/RT) of 35 kCal/mole , in good agreement with the latent heat of InCl 3 sublimation. At 250°C Eq. (27) predicts a maximum evaporation rate of nearly 45 ji...
text_only
18_plasma-etching-an-introduction_compress
For instance, small amounts of surface copper may be sputtered, especially if there is high ion energy. And the vapor pressure of Cu 3 C l 3 in equilibrium ![47_image_0.png](47_image_0.png) with an A1/A1C13 surface may differ from the vapor pressure of the pure chloride (because of solution and surface free energy e...
text_only
18_plasma-etching-an-introduction_compress
This effect is called feature sensitivity. Selectivity defines relative material etching rates in a plasma. The degree to which differential etching of one material relative to others is possible in a plasma is one of several factors that limits the fidelity of pattern transfer (Section IV.C). Selectivities may refe...
text_only
18_plasma-etching-an-introduction_compress
At first glance, reproducibility might appear to be more a matter of process control than an inherent process characteristic. However, etching equipment and processes sometimes have insidious "memory" or hysteresis effects that are difficult to control. The initial condition of the reactor can be influenced by accumula...
text_only
18_plasma-etching-an-introduction_compress
| ETCHING | SOURCE GAS | ADDITIVE | MATERIALS | MECHANISM | SELECTIVE | |----------------------------------|------------------------------|---------------|-----------------|---------------|-------------| | SPECIES | OVER ...
text_only
18_plasma-etching-an-introduction_compress
will be inversely proportional to the number of wafers in the reactor (see Chapter 2). Plasma etching has displaced most wet etching steps because it can deliver superior results according to these criteria. For instance, plasmas routinely achieve controlled anisotropic etching of fine features; whereas wet anisotrop...
text_only
18_plasma-etching-an-introduction_compress
## A. Linewidth Control Probably the single most desired result of a plasma process is faithful ![50_image_0.png](50_image_0.png) replication of the mask pattern in the film of semiconductor device. Submicron features can be formed with anisotropic etching chemistries and conditions. In practice the anisotropy br...
text_only
18_plasma-etching-an-introduction_compress
To preserve feature linewidth when highly doped polysilicon is etched by isotropic etchants such as fluorine or chlorine atoms, the sidewalls must be protected by an inhibitor film. Figure 26 illustrates the effects of adding a film-former, CC13F, to SF6 [35]. The undercut in a polysilicon feature beneath the resist m...
text_only
18_plasma-etching-an-introduction_compress
Inhibitor films also prevent lateral chemical attack during the etching of aluminum in chlorine-based plasmas. Since aluminum is normally passivated by a thin ( ~ 50 A) native oxide, which is impervious to chlorine, the etch chemistry must supply additional species that remove this layer. BC13 added to Cl 2 fulfills bo...
text_only
18_plasma-etching-an-introduction_compress
## B. Applying Isotropic An D Anisotropic Etching As processes were converted from liquid chemistries to dry etching, which permitted faithful replication of a mask, anisotropy was often accompanied by a loss of selectivity over the underlying substrate film. The anisotropic character of a process sometimes has to be ...
text_only
18_plasma-etching-an-introduction_compress
![55_image_0.png](55_image_0.png) This problem is aggravated when the first level conductor is a multi-thin composite, such as a suicide film over a doped polysilicon (I) layer. A typical example is shown in Fig. 30, where the first level runner is a layered silicide/poly I film. Unfortunately, during the definition ...
text_only
18_plasma-etching-an-introduction_compress
![56_image_0.png](56_image_0.png) ## C. Selectivit Y 1. Selectivity In Ion Etching Selectivity i n sputterin g almos t alway s decrease s wit h increasin g io n energ y (see Fig . 31) , whil e th e yield , o r sputterin g rate , increase s wit h energy . Although physica l sputterin g i s *relatively* unselective ...
text_only
18_plasma-etching-an-introduction_compress
![57_image_0.png](57_image_0.png) flux must be limited or there will be device damage and an intolerable degradation of selectivity. In contrast to chemical or ion-enhanced plasma etching, the product leaving a sputter-etched surface may be involatile. At low pressure when the mean free path is comparable to interel...
text_only
18_plasma-etching-an-introduction_compress
When resist is sputtered, the rapid removal rate at this critical "facet angle" causes a planar surface to develop (Fig. 33a, b) and propagate in this ![58_image_0.png](58_image_0.png) ![58_image_1.png](58_image_1.png) ![59_image_0.png](59_image_0.png) ![59_image_1.png](59_image_1.png) direction. As sputtering co...
text_only
18_plasma-etching-an-introduction_compress
## 2. Selectivity Analysis Selectivity, the etch rate ratio between materials, is a critical figure of merit. Conceptually, there are two kinds of selectivity that are needed, (1) selectivity for etching a substrate rather than the pattern mask (resist durability), and (2) etching selectivity between two material l...
text_only
18_plasma-etching-an-introduction_compress
To some extent, the resist mask thickness and selectivity for the film being etched are interchangeable degrees of freedom. Figure 36 shows a nominal 1.4 μ m thick positive resist film pattern applied over a 1.0 fim film of aluminum. The features beneath the aluminum layer produce a surface topography that causes the r...
text_only
18_plasma-etching-an-introduction_compress
$$(30)$$ $$|\mathbf{B}|=|d_{m}-d_{f}|=2\,y_{f}.$$ The absolute value sign makes this equation apply to both lines (B positive) and spaces (B negative) in Fig. 38. The degree of anisotropy A, is defined as $$\mathbf{A}=1-\left(\,R_{h}/R_{v}\right),$$ $$(31)$$ A = **1 -** *(Rh/Rv),* (31) ![62_image_0.png](62_ima...
text_only
18_plasma-etching-an-introduction_compress
From Fig. 39, an etched feature of dimension df , with equal lines and spaces, requires that a critical mask feature size $$d_{c}=d_{\mathrm{{\tiny~PTCH}}}-d_{m}=d_{\mathrm{{\tiny~PTCH}}}-|\mathbf{B}|-d_{f}$$ $$(33)$$ be printed in the resist. And for an etch process with anisotropy factor, A $\mathbf{a}=\mathbf{a...
text_only
18_plasma-etching-an-introduction_compress
$$t_{c}={\frac{y_{f}[1+\alpha]}{R_{f}[1-\beta]}}\,.$$ To allow for other sources of variation, the total etch time, / tot , is usually increased to include some "overetching," δ, which is usually expressed as a percentage of the final clearing time: $$t_{\mathrm{tot}}=t_{c}(1+\delta)=\frac{y_{f}}{R_{f}}\frac{[1+\alp...
text_only
18_plasma-etching-an-introduction_compress
$$S_{f}^{m}=\frac{\mathcal{V}_{f}}{\Delta}U_{f}^{m}\left[\cot\,\theta\,+\,\left[1\,-\,\mathbf{A}_{m}\right]\right],\tag{40}$$ ``` where A m is the anisotropy factor for mask attack and Uf m ...
text_only
18_plasma-etching-an-introduction_compress