![151_image_0.png](151_image_0.png) saturation at higher energies because of simultaneous etching. In general, the mixed layers in RIE are a few nanometers deep, which was good enough when structures to be etched had dimensions in the order of several tens of nanometers. Advanced devices, however, have critical dimens...
text_only
1_Atomic Layer Processing_semiconductor
Similar mixing layers are formed when etching silicon with fluorine- or bromine-containing species. Silicon fluoride is very volatile and thermal etching is possible. Therefore, fluorocarbon passivation gases are used to passivate sidewalls when etching silicon with fluorine-rich gases such as SF6 or NF3. For RIE of S...
text_only
1_Atomic Layer Processing_semiconductor
Redeposition of reaction products onto the etching surface influences RIE etching results greatly. Some etching processes such as silicon gate and isolation trench etch processes rely on redeposition of silicon-containing species for sidewall passivation to achieve vertical etching profiles. Nonuniform redeposition can...
text_only
1_Atomic Layer Processing_semiconductor
The MD simulation results in Figure 7.6 show that as the ion energy is increased, etching products are less saturated with halogen, which makes the products less volatile and increases the sticking probability (Gou et al. 2010). This is a general trend. The participation of reaction products in the process is very impo...
text_only
1_Atomic Layer Processing_semiconductor
Analysis of the sensitivity of the etching rate ER to the ratio of the two fluxes, the ion flux Ji and neutral flux Jn, using Eq. (7.4) reveals that the slope is least steep when both fluxes are of similar magnitude (after considering the other parameters in Eq. (7.4) such as neutrals sticking coefficient and ion energ...
text_only
1_Atomic Layer Processing_semiconductor
The ion-limited regime plays an important role in the etching of high aspect ratio features. The reason is that the angular distribution of neutrals is isotropic. They ![154_image_0.png](154_image_0.png) Figure 7.8 Illustration of neutral and ion-limited process regimes. ![154_image_1.png](154_image_1.png) collide ...
text_only
1_Atomic Layer Processing_semiconductor
![155_image_0.png](155_image_0.png) 0.15 **Figure 7.9** Graphical illustration of the ion-enhanced polysilicon etching with Cl and 100 eV Ar+. The etching yield for both physical sputtering and thermal etching of polysilicon are shown in the right-hand y-axis. Source: Chang et al. (1997). © 1997 AIP Publishing. surfa...
text_only
1_Atomic Layer Processing_semiconductor
Firstly, fast ions, either chemically reactive or nonreactive, can contribute to direct sputtering of bulk material if the energies are high enough and the neutral fluxes are too low to ensure continuous coverage. If the surface is completely covered by reactive neutrals, sputtering of bulk material has a low probabili...
text_only
1_Atomic Layer Processing_semiconductor
Etching of a chemically modified surface can also be initiated by electrons (Coburn and Winters 1979a) and photons (Shin et al. 2012). For an RIE process with all these components, the etching rate is determined by the contributions from the various species fluxes. To guarantee wafer to wafer and tool to tool repeatabi...
text_only
1_Atomic Layer Processing_semiconductor
The volume that is removed per reacting neutral vn is a function of the neutrals in weakening the bulk material. The binding energy of the chemically mixed layer is a function of the binding energy of the bulk material, the chemical reactivity of the adsorbing neutral species, and their concentration. In a simple fram...
text_only
1_Atomic Layer Processing_semiconductor
A special case of the influence of material properties on RIE rates is the etching of doped silicon. Heavily n-doped silicon etches faster, and p-doped silicon etches slower than undoped silicon in a fluorine plasma (Lee and Chen 1986; Winters and Haarer 1987). This doping effect is more pronounced in fluorine radical ...
text_only
1_Atomic Layer Processing_semiconductor
mechanism, i.e. Cabrera–Mott (CM) diffusion (Winters et al. 1983). Doping modifies the space charge at the surface. Field-enhanced diffusion in n-doped silicon drives the halogen ion into the bulk and enhances etching, while a repulsive field in p-doped silicon pushes the halogen ion to the surface and hence suppresses...
text_only
1_Atomic Layer Processing_semiconductor
The fluorocarbon polymer is not only an etch-inhibiting layer, but also the source of fluorine, which reacts with silicon and carbon, which reacts with oxygen. Schaepkens et al. found that SiO2, Si3N4, and silicon are covered with a several ![158_image_0.png](158_image_0.png) nanometer thin fluorocarbon film during ...
text_only
1_Atomic Layer Processing_semiconductor
Silicon is covered with a relatively thick fluorocarbon film of roughly 2–7 nm. The film thickness for Si3N4 is between SiO2 and silicon with about 1–4 nm. This difference in fluorocarbon film thickness and its correlation with etching rate allow etching SiO2 selectively to Si3N4 and silicon with fluorocarbon or hydrof...
text_only
1_Atomic Layer Processing_semiconductor
## 7.2.2 Ernu The complexity of the RIE etching mechanism creates severe engineering challenges to achieve etching rate uniformities that meet the requirements of advanced semiconductor devices. ALE etching technologies leverage self-saturation of the steps to achieve EPC uniformity across the wafer. Thermal and radic...
text_only
1_Atomic Layer Processing_semiconductor
## 7.2.3 Arde RIE is prone to ARDE as can be easily seen from Eq. (7.4). For a given point at the etching front inside a feature, the net ion and neutral fluxes entering Eq. (7.4) are dependent on the solid angle that has a line of sight to the plasma. There is also an energy dependence because the scattering probabil...
text_only
1_Atomic Layer Processing_semiconductor
With the emergence of etching of dielectric features with aspect ratios above 50 : 1, ion scattering is becoming an important contributing factor (Huang et al. 2019). Knudsen transport: The fundamentals of this neutral transport mechanism can be found in Section 2.8.1. The probability that a neutral atom or molecule r...
text_only
1_Atomic Layer Processing_semiconductor
Neutral shadowing: Under typical RIE process conditions with pressures between 0.1 and 100 mTorr, the mean free paths for collisions are much longer than characteristic dimensions of the etching structures. Therefore, neutral transport is in the molecular flow regime and gas-phase collisions can be neglected relative t...
text_only
1_Atomic Layer Processing_semiconductor
$\mathbf{\mu}_1=\nu_p$ For other portions of the profile besides the center of the bottom surface or for structures other than trenches or vias and for situations where sidewall etching is important, the solid angle expressions become more complicated (Gottscho et al. 1992). The implication from Eqs. (7.5) and (7.6) f...
text_only
1_Atomic Layer Processing_semiconductor
Simulations by Ingram revealed that the trajectories of normally incident positive ions can be perturbed by the local field structure during trench etching. This leads to an enhanced flux at the trench sidewalls (Ingram 1990). The surface potential evolves until the electron and ion fluxes are equal along all points of...
text_only
1_Atomic Layer Processing_semiconductor
Charging of polymer-covered sidewalls: In etching of SiO2 and Si3N4, the reactive species are fluorocarbon polymers. This leads to a special case of differential charging where the sidewall is a fluorocarbon polymer layer. Hayashi et al. conducted elegant experiments using capillary plates with aspect ratios of above ...
text_only
1_Atomic Layer Processing_semiconductor
Shading of polymer precursors: A commonly deployed technique to reduce or eliminate ARDE does not address the root cause but leverages the competing aspect ratio effects of etching vs deposition. RIE processes that use polymerizing gases to protect the sidewall or as reactive species are characterized by simultaneous o...
text_only
1_Atomic Layer Processing_semiconductor
Here, higher RF power is used to increase the energy flux of the etching species to the bottom of the feature and to balance profile and ARDE performance. ## 7.2.4 Selectivity RIE without significant deposition exhibits "intrinsic" selectivity. Intrinsic selectivity is a function of "excess" removal energy, which can...
text_only
1_Atomic Layer Processing_semiconductor
Figure 7.15 illustrates this conceptual framework for etching selectivity. Thermal etching and thermal isotropic ALE have the highest intrinsic selectivity because the excess energy is close to zero. Infinite intrinsic selectivity is possible. Radicals are less selective because they have unpaired electrons. They can o...
text_only
1_Atomic Layer Processing_semiconductor
Deposition reactions are frequently used to boost selectivity. We described this approach for directional ALE with reactive layer deposition in Section 6.1.3 where we discussed the C4F6/Ar+ of SiO2. In continuous RIE, the deposition and removal reactions proceed simultaneously. The origin of selectivity is enhanced pol...
text_only
1_Atomic Layer Processing_semiconductor
Another example of deposition-enhanced selectivity is etching of silicon selectively to silicon oxide. A typical application is patterning of polysilicon gates with a few nanometer thin gate oxide stop layer. Toward the end of the 1990s, Moore's Law drove the thickness of gate oxides to less than 50 nm. At that time, t...
text_only
1_Atomic Layer Processing_semiconductor
Gate oxide lifetime is shorter when silicon loading increases. This is the result of oxygen consumption by silicon and a reduction of protective polymer deposition onto the exposed gate oxide. ## 7.2.5 Profile Control So far, we discussed performance metrics that painted a rather mixed picture for RIE compared to the...
text_only
1_Atomic Layer Processing_semiconductor
The profile of a sputtered feature is determined by the angular distribution of the sputtering yield. The lower the sputtering yield is for large incidence angles, the more tapered the profile will be. Hence, tapered profiles can be achieved using chemical and chemically enhanced sputtering. Most RIE processes, however...
text_only
1_Atomic Layer Processing_semiconductor
The same process chemistry can passivate the sidewall also by CVD-like deposition from the plasma. This mechanism is depicted as "plasma deposition" in Figure 7.17. It relies on material from the wafer to form passivation species in the plasma. In the case of silicon RIE with chlorine and oxygen, the silicon can ![167...
text_only
1_Atomic Layer Processing_semiconductor
Etching of features involves a mask, and the etching selectivity for most mask materials is finite. Hence, etched mask material will also enter the plasma region and participate in the deposition process. Depending on the kind of mask material and the selectivity, this may influence the sidewall thickness and compositi...
text_only
1_Atomic Layer Processing_semiconductor
SiO2 SiO2 ![169_image_1.png](169_image_1.png) the passivation layer is increased from 28 to 40 at.%, which indicates a thinner passivation layer. Next, we will discuss plasma passivation in more detail. In particular, we will analyze why it is possible to protect a vertical surface via plasma passivation while etchi...
text_only
1_Atomic Layer Processing_semiconductor
Another sidewall passivation mechanism is direct line of sight redeposition of nonvolatile etching products. We discussed this mechanism in the context of profile performance of directional ALE (see Section 6.2). Figure 6.24 illustrates that the profile becomes less bowed and eventually tapered when redeposition of spu...
text_only
1_Atomic Layer Processing_semiconductor
Besides synergistic etching as expressed by Eq. (7.4), RIE mechanisms can include simultaneous thermal and radical etching as well as direct physical and chemical sputtering. Sidewall passivation must prevent lateral etching by radicals and reactive neutrals as well as from ion bombardment. Etching of aluminum in a chl...
text_only
1_Atomic Layer Processing_semiconductor
## 7.2.5.2 Selection Of Etching Species In this approach to achieve vertical profiles, isotropic etching caused by radical or thermal etching is suppressed by selecting etching gases, which form less volatile reaction products (Coburn and Winters 1979b). Coburn gives the example of etching of silicon with fluorine-, c...
text_only
1_Atomic Layer Processing_semiconductor
Based on this observation, Coburn suggested to use mixtures of fluorine, chlorine, and bromine gases to achieve vertical profiles as schematically shown in Figure 7.21. This approach is widely used in the development of RIE processes that use halogen gases. ![171_image_0.png](171_image_0.png) ## 7.2.5.3 Temperature ...
text_only
1_Atomic Layer Processing_semiconductor
Source: Tachi et al. (1988). © 1988 AIP Publishing. etching cannot be prevented even at temperatures below −100 ∘C and roughly 10% of oxygen was added to SF6 to provide better sidewall passivation (Bartha et al. 1995). Bartha et al. suggested that the results by Tachi and coworkers were influenced by small amounts of...
text_only
1_Atomic Layer Processing_semiconductor
Let us first discuss physical sputtering. The ions in RIE carry energies between several ten to several thousand electron volts and can cause physical sputtering in a neutral limited regime. Upon impact onto the surface, these ions create a collision cascade in the solid material. The temperature of the atoms in the co...
text_only
1_Atomic Layer Processing_semiconductor
Therefore, the etching rate of pure synergistic RIE with dominant radical adsorption (without parallel thermal or radical etching or deposition processes) is most likely not temperature sensitive. Based on these arguments, we can exclude physical, chemical, and chemically enhanced sputtering as the primary root cause ...
text_only
1_Atomic Layer Processing_semiconductor
Most RIE processes deploy deposition processes to passivate the sidewall of the etching structure. The deposition processes can be classified into CVD-type plasma deposition and line-of-sight sputtering. What is the temperature sensitivity of these deposition processes? In the case of line-of-sight sputtering, the reac...
text_only
1_Atomic Layer Processing_semiconductor
In conclusion, RIE profiles can be very effectively tuned using wafer temperature. This is the result of accelerated lateral thermal and radical etching and suppression of CVD deposition rates. This has profound implications for RIE reactor design. Because the etching profile is determined by the flux of passivating ...
text_only
1_Atomic Layer Processing_semiconductor
Therefore, the discussion in section 7.2.5. on profile tuning is directly applicable to CD control in RIE. CD control is essentially sidewall passivation thickness control across the chip, across wafer, and wafer to wafer. The difference between the mask CD and the feature CD is called CD bias or ΔCD. From the discuss...
text_only
1_Atomic Layer Processing_semiconductor
The preferred method of measuring CDs in the manufacturing of integrated circuits (ICs) is top down scanning electron microscopy (SEM) or CD-SEM, which produces a 2D image. The mask areas and the etched features are represented by lighter or darker colors or gray shades. The edge of a line or hole is defined by the bri...
text_only
1_Atomic Layer Processing_semiconductor
The difference between the chip layout, which is the intent of the designer, and the final etch CD is also called edge placement error (EPE). The factors that contribute to EPE include systematic errors from lithography and etching. These systematic errors must be considered in the design of the mask. In the case of sy...
text_only
1_Atomic Layer Processing_semiconductor
![176_image_0.png](176_image_0.png) Still, the isolated feature will have a larger CD because the area from which nonvolatile sputtered deposition species originate is larger for isolated features. A larger surface area is exposed to etching next to an isolated feature compared to a dense feature. In the case of etch...
text_only
1_Atomic Layer Processing_semiconductor
When CF4 is added to the process, the sidewall passivation changes from silicon oxychloride and oxybromide to carbon based (see Figure 7.20). The carbon-based passivation layer is thinner while still providing protection from lateral etching. This thinner and stronger passivation layer allows achieving zero CD microloa...
text_only
1_Atomic Layer Processing_semiconductor
## 7.2.7 Surface Smoothness RIE processes are characterized by the presence of a mixed or selvage layer. MD simulations by Graves and Humbird for etching of silicon with fluorine (Graves and Humbird 2002) and Feil et al. for etching of silicon with chlorine (Feil et al. 1993) led to the conclusion that the selvage lay...
text_only
1_Atomic Layer Processing_semiconductor
The initial mask for any stack is the photoresist pattern, which is characterized by typical features as shown in Figure 7.27. They are crevices with high spatial frequencies of larger than 1/50 nm−1, resist feet for medium spatial frequencies between 1/50 and 1/200 nm−1, and bulk features with low spatial frequencies ...
text_only
1_Atomic Layer Processing_semiconductor
![179_image_0.png](179_image_0.png) microloading/LWR trade-off can be overcome by separating photoresist etching and deposition reactions. Source: Lill et al. (2014). Goldfarb et al. demonstrated that isotropic resist roughness found on the resist walls after the lithographic step becomes anisotropic during the etchin...
text_only
1_Atomic Layer Processing_semiconductor
A proven approach to reduced roughening of the photoresist includes plasma treatment steps (Pargon et al. 2009; Azarnouche et al. 2013). Pargon et al. studied the effect of HBr and Ar plasmas on the composition of 193 nm photoresist. They were able to distinguish the effects of vacuum ultraviolet (VUV, 110–210 nm) ligh...
text_only
1_Atomic Layer Processing_semiconductor
As the result of cross-linking and removal of hydrogen- and oxygen-containing ester and lactone groups, HBr plasma is established as a preferred method to increase resist etch resistance and also to significantly reduce the LWR/LER of 193 nm photoresist patterns. Azarnouche et al. compared HBr plasma and VUV treatment...
text_only
1_Atomic Layer Processing_semiconductor
The etched structures were measured by means of AFM. The etching depth was found to be one of the main control parameters for buckling. For the same width, buckling is more pronounced for the lines that are patterned deeper and have larger aspect ratios. The height of the TiN mask and the Young's modulus of the ILD, an...
text_only
1_Atomic Layer Processing_semiconductor
![181_image_0.png](181_image_0.png) buckling is suppressed when the RF power in the RIE process is reduced. Weak mask materials with low modulus can be stabilized by encapsulating it with a low stress film in the RIE reactor before or during etching. If the film has tensile stress, line buckling can even be improved. ...
text_only
1_Atomic Layer Processing_semiconductor
The LER/LWR challenges we discussed so far are even more pronounced for extreme ultraviolet (EUV) resists. High-frequency LER and LWR of EUV resists is a function of exposure dose due to stochastic effects. Exposure time in EUV is extremely expensive and hence etching and materials solutions are needed to repair high-f...
text_only
1_Atomic Layer Processing_semiconductor
Classification into conductor and dielectric etch applications is still used today; however, the resistivity of the material is not a definitive property for classification. For instance, silicon nitride is frequently etched in both conductor and dielectric etch tools. High aspect ratio silicon vias are etched primaril...
text_only
1_Atomic Layer Processing_semiconductor
Aspect ratio: It turns out that plasma requirements for patterning of 4 to 10 : 1 aspect ratio features with extreme CD control and conductor etch applications overlap to a large extend. At the same time, CCP tools emerged as the tools of choice to etch high aspect ratio (50 : 1 and higher) trenches and holes. This cla...
text_only
1_Atomic Layer Processing_semiconductor
The classification by IC manufacturing module is important to prevent metal cross-contamination. In the following, we will discuss important etching applications with unique requirements. ## 7.3.1 Patterning 7.3.1.1 Self-Aligned Patterning The goal of most etching processes is to transfer a pattern generated by lith...
text_only
1_Atomic Layer Processing_semiconductor
Because carbon cannot be etched selectively with resist, this required a thin dielectric layer on top of the carbon, which also acted as a DARC for lithography. Because DARC layers contained nitrogen, which interacts with the resist to form a foot at the bottom of the profile, organic antireflective coating where intro...
text_only
1_Atomic Layer Processing_semiconductor
The complete pattern then emerges when all lithography and etching processes are completed. This is a brute force method to generate features beyond the resolution of lithography and is called Litho-etch-Litho-etch (LELE). It is obviously expensive and also suffers from the challenge to align the different parts of the...
text_only
1_Atomic Layer Processing_semiconductor
![185_image_0.png](185_image_0.png) At the core of self-aligned multi-patterning is the sidewall image transfer (SIT) or spacer patterning technique. Here, a first line is patterned with 193 nm immersion lithography. The pitch, which is the sum of the line width and space between the lines, is twice the desired final ...
text_only
1_Atomic Layer Processing_semiconductor
Let us now discuss the requirements for each step in more detail from an etching technology point of view. Depending on whether the mandrel is made of carbon or polysilicon, oxygen-, or halogen-based processes are used. The aspect ratio of the final mandrel is only around 3 to 1. Hence, high-density plasmas are typical...
text_only
1_Atomic Layer Processing_semiconductor
In the case of a polysilicon mandrel, typical RIE processes are halogen based. If chlorine or hydrogen bromide gases are used, selectivity to the mask is achieved via plasma deposition of silicon oxychloride and oxybromide reaction products. These compounds also deliver sidewall passivation. For fluorine-based plasma c...
text_only
1_Atomic Layer Processing_semiconductor
Negative tone spacer double patterning is preferred for patterning of structures where the space between the lines is more important. Examples are trenches. SADP with negative spacer tone is schematically depicted in Figure 7.33. The bifurcation of SADP into positive and negative spacer tone schemes is implemented afte...
text_only
1_Atomic Layer Processing_semiconductor
In the negative tone spacer approach, the gap between the spacers is filled and polished back. Typically, the fill material is the same as the mandrel material. If the fill material is any material other than the mandrel, subsequent cuts can be selective to either the mandrel or the gap fill material. This allows a sel...
text_only
1_Atomic Layer Processing_semiconductor
SADP can also be used to pattern hole masks. Figure 7.34 shows that square and hexagonal hole arrangements can be obtained by repeating the SADP process twice. In the case of hexagonal layout, the two SADP patterns are rotated by 60∘ with respect ![188_image_0.png](188_image_0.png) ![188_image_1.png](188_image_1.png...
text_only
1_Atomic Layer Processing_semiconductor
## 7.3.1.2 Extreme Ultraviolet (Euv) Lithography Extreme ultraviolet (EUV) scanners use a wavelength of 13.5 nm, which is generated in a laser-driven tin plasma light source. The short wavelength of EUV lithography enables patterning of lines and spaces with sub-60 nm pitch without SADP. Sub-20 nm lines and spaces ca...
text_only
1_Atomic Layer Processing_semiconductor
These processes are being run in ICP/TCP reactors either standalone or in situ with subsequent mask etches. Alternating selective carbon deposition and smoothening with directional ALE show promising performance (Wise and Shamma 2018). This is an example of how the smoothening effect of ALE is used to aid with the imp...
text_only
1_Atomic Layer Processing_semiconductor
![190_image_0.png](190_image_0.png) flow from the top of the reactor. Figure 7.36 illustrates the complexity of the reactant and reaction product fluxes in the reactor because of the blockage by the wafer (Kiehlbauch and Graves 2003). The model in Figure 7.36 assumes a pressure of 50 mTorr, 50 W of inductive RF power,...
text_only
1_Atomic Layer Processing_semiconductor
Based on these discussions we can see that the CD bias uniformity pattern across the wafer can be flipped just by changing the pressure within a range that is entirely covered, for instance, by polysilicon gate main and overetches. The main etch may be conducted at 4–5 mTorr and the overetch at 50 mTorr or thereabout. ...
text_only
1_Atomic Layer Processing_semiconductor
## 7.3.2 Logic Devices 7.3.2.1 Fin Etch The evolution from planar transistor to fin field effect (FinFET) and gate-all-around (GAA) transistors is illustrated in Figure 7.37. The formation of a FinFET transistor includes two important RIE applications, Fin etch and FinFET gate etch. First, we will discuss Fin etch. T...
text_only
1_Atomic Layer Processing_semiconductor
Modeling results of a silicon Fin etch are shown in Figure 6.24 and germanium fins etched with Directional Cl2/Ar ALE are depicted in Figure 6.25. These examples illustrate some of the main challenges in Fin etch: ARDE, profile shape, and profile loading. Since the etching materials are silicon and germanium, the etchi...
text_only
1_Atomic Layer Processing_semiconductor
Advanced RIE reactors offer in situ dielectric atomic layer deposition (ALD) capability. When periodic passivation is used to protect the top fin profile, it is important to tune the passivation breakthrough step carefully to avoid profile discontinuities. Even though Fin etch is a high aspect ratio etch, ion energy m...
text_only
1_Atomic Layer Processing_semiconductor
of the defects is about 1 nm. This means that for a 10 nm wide Fin, the model predicts that the damaged region constitutes about 20% of the entire fin width even at a fairly low ion energy of only 200 eV. As the fin width is decreased and the ion energy is increased to etch fins with higher aspect ratios, the ratio of ...
text_only
1_Atomic Layer Processing_semiconductor
## 7.3.2.2 Gate Etch Etching of transistor gates has changed tremendously with the evolution from planar to FinFET gates as illustrated in Figure 7.37. One of the most important performance requirements of the gate etch application is CD control because the length of the gate is determined by the CD and LWR/LER of the...
text_only
1_Atomic Layer Processing_semiconductor
Selectivity to gate oxide is very important. In fact, the requirement is not just to stop on only a few Angstrom of gate oxide, but to avoid damage of the crystalline silicon underneath. Plasma oxidation of the silicon substrate occurs during overetching with HBr/O2 RIE. This silicon oxide is removed in subsequent wet ...
text_only
1_Atomic Layer Processing_semiconductor
The replacement of silicon with metals eliminates the so-called depletion region in the gate just above the gate oxide. This depleted region in a semiconducting gate acts like a thicker gate oxide when the gate voltage is applied. Thus, the implementation of gate metals reduces the effective gate oxide thickness. High...
text_only
1_Atomic Layer Processing_semiconductor
![195_image_0.png](195_image_0.png) the same time. Plasma using BCl3 can etch HfO2 selectively to silicon and silicon oxide, but the bias power must be controlled carefully to achieve selectivity as shown in Figure 7.40. In this experiment, a bias power of only 5 W was needed to achieve an etching rate of 30 Å/min and...
text_only
1_Atomic Layer Processing_semiconductor
Because of etching challenges and limited materials integration flexibility in the "gate first" approach, the "gate last" integration dominated the industry beyond the 45 nm node. This choice turned out to be the right one to enable the next change in gate integration, the change from planar to FinFET gates (see Figure...
text_only
1_Atomic Layer Processing_semiconductor
Spacer etch was one of the first applications where Si3N4 was etched (Regis et al. 1997). It is an archetypical Si3N4 RIE application. Si3N4 is also etched in fluorocarbon plasma such as silicon oxide. However, it does not contain oxygen to consume carbon. Therefore, Si3N4 etching requires hydrogen addition to the pla...
text_only
1_Atomic Layer Processing_semiconductor
demonstrated an all-dry directional ALE process with removal by a capacitively coupled fluorine plasma with SF6 or NF3 feed gas instead of diluted HF (Sherpa and Ranjan 2017). ## 7.3.2.4 Contact Etch Contact etching is a very critical application. Every single contact must be open for the logic chip to function and t...
text_only
1_Atomic Layer Processing_semiconductor
In the late 1990s, further scaling of logic and also DRAM devices reduced the space between gate lines to such a degree that the contact hole started to overlap with the gate, either by design or by misalignment. The resulting contact was called a self-aligned contact. In such a contact the etch exposes the corner of t...
text_only
1_Atomic Layer Processing_semiconductor
The selectivity requirements increased further with the advent of FinFET gates. When landing on fins, their corners are exposed. To decrease contact resistance, epitaxial silicon or SiGe is grown around the fins as illustrated in the right panel in Figure 7.41. Selectivity to SiGe is lower than to silicon. Epitaxy for...
text_only
1_Atomic Layer Processing_semiconductor
## 7.3.2.5 Beol Etch Among all the logic etch applications, BEOL etching underwent one of the most dramatic changes. Before the turn of the century, logic device metallization was realized with aluminum, which was etched directly with a resist mask or a hardmask. Aluminum etches readily with chlorine. The isotropic et...
text_only
1_Atomic Layer Processing_semiconductor
A so-called copper damascene interconnect approach was developed as an alternative and transformed into high-volume production. It is the integration approach that is used in all logic devices today. There are two embodiments of damascene interconnect integration: "trench first" and "via first." Simplified process flow...
text_only
1_Atomic Layer Processing_semiconductor
Besides the etching steps, BEOL integration involves other processing steps such as post etch cleaning, low-k sealing, barrier deposition, copper fill, and CMP. ![199_image_0.png](199_image_0.png) A detailed description of the different integration schemes and challenges goes beyond the scope of this book. The intere...
text_only
1_Atomic Layer Processing_semiconductor
Therefore, the approach to porous low-k etching is to use heavy sidewall passivation to close the pores. Porous low-k materials are typically etched in a C4F8-based process in dual-frequency CCP reactors. C4F8 is a carbon-rich gas that effectively generates fluorocarbon polymers in plasmas as discussed in section 7.3.2...
text_only
1_Atomic Layer Processing_semiconductor
Atomic layer etching has been used to extend the BEOL RIE process (Lutker-Lee et al. 2019). Lutker-Lee et al. demonstrated that directional ALE successfully suppressed RIE while keeping low-k damage to a minimum. In addition, the ALE showed improved hardmask selectivity and resulted in lower line edge pattern roughness...
text_only
1_Atomic Layer Processing_semiconductor
Advanced deep trench etch processes were able to achieve aspect ratios of 80 : 1 (see Figure 2.13). The challenge for deep silicon etching is the risk of lateral etching by fluorine radicals. High aspect ratio silicon etching of DRAM capacitors was conducted in CCP reactors in most cases with enhancement of the plasma ...
text_only
1_Atomic Layer Processing_semiconductor
The trade-off between lateral etching and too much passivation also exists in high aspect ratio etching of silicon oxide to form stack capacitors. While sidewall passivation breakthrough in the case of silicon holes has catastrophic consequences, the impact on oxide trenches is more gradual in the form of bowing. The r...
text_only
1_Atomic Layer Processing_semiconductor
High aspect ratio silicon oxide capacitor etching is the processing technology that enables the DRAM roadmap today. Silicon oxide capacitors are etched with C4F8and C4F6-based chemistries in double- or triple-frequency CCP reactors. SiO2 capacitor cell etching is the archetypical high aspect ratio dielectric etching ap...
text_only
1_Atomic Layer Processing_semiconductor
It is predicted that this patterning approach will be one of the first steps that will be replaced by EUV lithography. The critical technical challenges of high aspect ratio dielectric etching are etching rate and ARDE, profile performance including necking, bowing, hole distortion, and twisting, as well as mask selec...
text_only
1_Atomic Layer Processing_semiconductor
Etching of high aspect ratio features into dielectrics such as SiO2 and Si3N4 faces the challenge to deliver thermal radicals to the etching front. The transport mechanism of these radicals is Knudsen transport (see Section 2.8.1). Owing to the limits of vacuum conductance, the probability of neutral radicals reaching ...
text_only
1_Atomic Layer Processing_semiconductor
The majority of the reactive ions generated in C4F6 and C4F8 plasmas are CF2 + and CF3 +. Etching of SiO2 has been studied with energy-controlled and mass-selected beams of CF2 + and CF3 + ions (Toyoda et al. 2004) and simulated by a quantum chemical MD model of fast radical interactions (Ito et al. 2013, 2014). Accor...
text_only
1_Atomic Layer Processing_semiconductor
Huang et al. conducted computational investigations that confirm this mechanism. They simulated the plasma and used the resulting fluxes and energies to investigate the profile evolution for 80 : 1 AR features in SiO2. The feed gases were argon, C4F8, and oxygen. The plasma was energized by three CCP-coupled RF frequen...
text_only
1_Atomic Layer Processing_semiconductor
The flux of fast neutral to the etching front is about two to three times higher than the ion flux for aspect ratios above 5. This is because ions neutralize and thus contribute to the neutral flux. The flux of fast neutrals more than doubles with increasing aspect ratios from 1 to 5. This means that the fast neutral t...
text_only
1_Atomic Layer Processing_semiconductor
use the following simplified relationship for the energy and angular distribution of scattered ions and fast neutrals in their three-dimensional Monte Carlo feature profile model (Huang et al. 2019): ![205_image_0.png](205_image_0.png) $$E(\theta)_{\rm out}=E_{\rm in}\left(\frac{E_{\rm in}-E_{1}}{E_{2}-E_{1}}\right)\...
text_only
1_Atomic Layer Processing_semiconductor
Figure 7.45 shows the ion energy distributions of the scattered ions. Near zero energy loss is observed for large incoming angles in of 88∘ and 89∘. Ions that have the same impact angles but are scattered with a larger outgoing angle lose energy as manifested by the long tail. For incoming angles of 80∘, all ions lose ...
text_only
1_Atomic Layer Processing_semiconductor
As the AR increases, conductance limits of the isotropic thermal radicals reduce their fluxes into the feature and the etching mechanism changes. The contribution of physical and chemical sputtering increases because the fluxes of energetic species to the etch front surpass those of the conduction constrained CFx and C...
text_only
1_Atomic Layer Processing_semiconductor
Kim et al. developed a semiempirical profile simulator and showed that the net deposition rate of polymer on the sidewall defines the amount of necking. Upon exposure to plasma, ion impact causes erosion of the mask and a primary facet forms as a result as shown in Figure 7.47. Mask erosion is strongly influenced by th...
text_only
1_Atomic Layer Processing_semiconductor
The necking and bowing, which are derived from the simulated profiles, are shown in Figure 7.49 (Kim et al. 2007). Necking is defined as (top CD - neck CD)/top CD and bowing as (bow CD − top CD)/top CD. Top CD is the width of the opening at the top of the etched oxide feature. Necking increases continuously ![209_imag...
text_only
1_Atomic Layer Processing_semiconductor
As the neutral depositor flux increases, necking increases. More ions are reflected and cause bowing. As neutral depositor flux increases further, the bowing starts to decrease. The sidewall below the neck becomes well passivated with polymer. This nonlinear relationship between deposition precursor flux and bowing is ...
text_only
1_Atomic Layer Processing_semiconductor