text stringlengths 1 2k | question stringclasses 1
value | answer stringclasses 1
value | label stringclasses 1
value | origin stringclasses 18
values |
|---|---|---|---|---|
The sputtering rate is directly proportional to the binding energy according to Eq. (2.8). In comparison, amorphous silicon is a "weak" material with a binding energy of 4.7 eV.
Figure 7.50 shows Monte Carlo simulation results of freestanding lines of carbon and silicon after 1 keV argon ion bombardment. The model is ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
It turns out that these conclusions change when the mask forms a dense array of lines (see Figure 7.51). In the model, the sticking coefficient for the redeposition was selected to be one. Deposition from the plasma was not considered in these simulations. Necking is caused by redeposition of mask material. Figure 7.51... | text_only | 1_Atomic Layer Processing_semiconductor | ||
So far, we discussed the relationship between necking and bowing as well as the role of the hardmask material. Next, we will explore the critical high aspect ratio etching metrics of twisting and distortions. The definitions for twisting and distortion are illustrated in Figure 7.52. The footprint of the holes on the b... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 7.53 shows experimental results for distortion and twisting. Twisting is visible as the shift of the hole center from the layout matrix lines (Kim et al. 2015).
One root cause hypothesis for twisting and distortions that is frequently discussed is asymmetric ion scattering. The idea is that the effect of ion sc... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Miyake et al. calculated the incident ion flux distributions at the hole bottom for axisymmetric and non-axisymmetric necking of a cylindrical hole (Miyake et al.
2009). In the case of non-axisymmetric necking, the imbalance of ion flux in the bottom of the hole brakes the etching symmetry in the bottom part of the ho... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 7.57 confirms the relationship between necking widths for trench structures we observed for holes in Figure 7.55. The data in Figure 7.57 show the benefit of higher ion energies to extend the twisting free depth. Higher ion energies are therefore one of the main technology drivers for high aspect ratio dielectri... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Similar calculations can be conducted for charged holes. The differences between holes and trenches is that the charged and non-charged sidewall is shunted by the circular sidewall. The conductance of the sidewall polymer is therefore important

for sidewall charging induced twistin... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Shimmura et al. used an on-wafer monitoring device to measure the charging potential in SiO2 contact holes (Shimmura et al. 2004). The potentials of the SiO2 contact hole top and bottom surfaces were measured during argon plasma exposure with and without deposited fluorocarbon film in the holes. The fluorocarbon films ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
For larger aspect ratios, the cross section of the feature deviates from a circular profile. An overetch tends to round previously noncircular features and removes the anomalies caused by the tapered etch front. The rounding of the feature by overetch is less effective with charging. Charging aggravates feature distort... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The second critical high aspect ratio dielectric etch is the isolation trench etch, which separates blocks of memory cells from each other. The channel and the isolation trench are etched into the alternating layers. Finally, the devices have to be connected to the control logic, which is why contact etches are needed.... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The other difference is that the CDs of the holes are different. The CDs are about 70 nm for OPOP and 100 nm for ONON while DRAM capacitor cells have a CD of 20–30 nm. The reason for larger CDs in 3D NAND devices is that there must be enough space to fit the device into the channel.
Despite significantly larger CDs, t... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The hypothesis is that if the etching front between a slowly and fast etching layer is broken though off center, the etching rate will accelerate in the faster etching layer. This should amplify the asymmetry and potentially introduce twisting and distortions.
Figure 7.62 shows Monte Carlo modeling results for etching... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The high aspect ratio contact etch process patterns either the two dual material stack or SiO2 depending on the type of contact. The contact to the staircase is patterned in SiO2. Selectivity is the largest challenge because the etching depth varies step to step (see Figure 7.61).
## 7.3.4 Emerging Memories
One of th... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Table 7.1 shows a list of emerging memory devices and typical materials used in their implementation as well as their use cases.
| Emerging memory | Metals | Metal oxides |
|---------------------------------------|---------------------------|-----------------... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 7.63 Schematic illustration of programming and reading of PCM
cells. Source: Wong et al. (2010).
© 2010 IEEE.

## 7.3.4.1 Phase Change Memory (Pcm)
One of the first storage class memories that is produced in large volume is phase change memory (PCM). It is also called phase... | text_only | 1_Atomic Layer Processing_semiconductor | ||

via selective removal of volatile species and implantation of species from the plasma. Because germanium, antimony, and tellurium can oxidize in air, the handling of the wafers after etching is critical and different from other etching applications. Encapsulation with a hermetic fil... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The stoichiometry of GST and OTS must be preserved after etching because small changes can impact the switching temperature of GST and OTS as well as other electrical parameters. Even if only a few nanometers of the sidewall material is altered, the scalability to CDs of 20 nm and below can be at risk because diffusion | text_only | 1_Atomic Layer Processing_semiconductor | ||
| Ge | Sb | Te | Se | As | | | | | | |
|-----------------------------------------|---------|----------|---------|----------|-------|------|-------|-----|-------|-------|
| Boiling | Boiling | ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
| GeCl2 | 450 | SbCl5 | 140 | [TeCl4]4 | 387 | | | | | |
| Br | GeBr4 | 186 | SbBr3 | 286 | TeBr2 | 339 | SeBr4 | N/A | AsBr3 | 221 |
| GeBr2 | 150 | [TeB... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 7.65 Fractional crystallization vs laser pulse heating time for nitrogen-doped GST samples as a function of surface treatment. Source: Washington et al. (2011). © 2011 AIP
Publishing.

can change the bulk composition. The effect of a change in GST stoichiometry is shown in Fi... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The use of halogens in RIE and neural beam etching of GST and OTS has been widely studied (Yoon et al. 2005; Kang et al. 2008, 2011a,b; Li et al. 2016; Park et al.
2019; Altieri et al. 2018; Canvel et al. 2019, 2020). A review of challenges and innovations of dry etching, wet cleaning, encapsulation, and the interacti... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Among the halogen gases, HBr was found to damage GST the least. This is most likely the result of bromine being less reactive and the etching effect of hydrogen.
The highest halogen surface concentration was found for CF4 (Kang et al. 2011a; Li et al. 2016). CF4 gave more vertical profiles compared to chlorine because... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The etched GST and OTS surfaces are prone to oxidation in atmosphere.
Figure 7.67 shows oxygen concentration on a GST surface as a function of time and oxygen pressure (Shen et al. 2019). The GST surface was cleaned with an argon ion

Figure 7.66 Cross-sectional images and the TEM/... | text_only | 1_Atomic Layer Processing_semiconductor | ||


Oxidation shifts the onset of crystallization of amorphous GST to higher temperatures as shown in Figure 7.69. Furthermore, in the absence of oxidation, nucleation occurs inside the volume of the Ge2Sb2Te5 film, while in oxidized films heterogene... | text_only | 1_Atomic Layer Processing_semiconductor | ||
OxRAM devices are much more amiable to etching because the switching materials are metal oxides such as TiOx, ZrOx, HfOx, VOx, NbOx, TaOx and others. The fact that the metals are in the oxidized state suggests that they should generally react with halogens and form volatile by-products. The stack thickness is in the ra... | text_only | 1_Atomic Layer Processing_semiconductor | ||
P7.7 What is the implication of the formation of a mixed layer on intrinsic selectivity of RIE?
P7.8 Using Eq. (2.2), explain why temperature is an effective knob to compensate ERNU caused by neutral flux nonuniformities in RIE reactors.
P7.9 Explain the relationship between sidewall passivation etching resistance an... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Berry, I.L., Park, J.C., Kim, J.K. et al. (2017). Patterning of embedded STT-MRAM
devices: challenges and solutions. *ECS and SMEQ Joint International Meeting 2018*,
Cancun, Mexico.
Berry, I.L., Kanarik, K.J., Lill, T. et al. (2018). Applying sputtering theory to directional atomic layer etching. *J. Vac. Sci. Technol... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Chang, J.P., Arnold, J.C., Zau, G.C.H., and Shin, H.S. (1997). Kinetic study of low energy argon ion-enhanced plasma etching of polysilicon with atomic / molecular chlorine.
J. Vac. Sci. Technol., A 15: 1853–1863.
Chang, J.P., Mahorowala, A.P., and Sawin, H.H. (1998). Plasma-surface kinetics and feature profile evolu... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Cunge, G., Inglebert, R.L., Joubert, O., and Vallier, L. (2002). Ion flux composition in HBr/Cl2/O2 and HBr/Cl2/O2/CF4 chemistries during silicon etching in industrial high-density plasmas. *J. Vac. Sci. Technol., B* 20: 2137–2148.
Desvoivres, L., Vallier, L., and Joubert, O. (2001). X-ray photoelectron spectroscopy i... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Gottscho, R.A., Jurgensen, C.W., and Vitkavage, D.J. (1992). Microscopic uniformity in plasma etching. *J. Vac. Sci. Technol., B* 10: 2133–2147.
Gottscho, R.A., Cooperberg, D., and Vahedi, V. (1999). The black box illuminated.
Workshop on Frontiers in Low Temperature Plasma Diagnostics III (LTPD), Saillon, Switzerlan... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Technol., A 37: 031304 1–26.
Huard, C.M., Zhang, Y., Sriraman, S. et al. (2017). Role of neutral transport in aspect ratio dependent plasma etching of three-dimensional features. *J. Vac. Sci. Technol., A*
35: 05C301 1–18.
Huard, C.M., Sriraman, S., Paterson, A., and Kushner, M.J. (2018). Transient behavior in quasi-... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Jin, W., Vitale, S.A., and Sawin, H.H. (2002). Plasma–surface kinetics and simulation of feature profile evolution in Cl2+HBr etching of polysilicon. *J. Vac. Sci. Technol., A* 20:
2106–2114.
Joubert, O., Oehrlein, G.S., and Surendra, M. (1994). Fluorocarbon high density plasma.
VI. Reactive ion etching lag model for... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Kim, J.K., Lee, S.H., Cho, S.I., and Yeom, G.Y. (2015). Study on contact distortion during high aspect ratio contact SiO2 etching. *J. Vac. Sci. Technol., A* 33: 021303 1–6.
Kanarik, K.J., Tan, S., and Gottscho, R.A. (2018). Atomic Layer Etching: Rethinking the art of etching. *J. Phys. Chem. Lett.* 9: 4814–4821.
Kur... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Lill, T., Kamarthy, G., Eppler, A. et al. (2014). Advanced patterning: plasma etch challenges and solutions. *Presentation at the SPIE Advanced Lithography Conference*,
San Jose, CA, USA.
Lill, T., Kanarik, K.J., Tan, S. et al. (2018). Benefits of atomic layer etching (ALE) for material selectivity. *ALD/ALE conferenc... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Metzler, D., Li, C., Engelmann, S. et al. (2016). Fluorocarbon assisted atomic layer etching of SiO2 and Si using cyclic Ar/C4F8 and Ar/CHF3 plasma. J. Vac. Sci. Technol.,
A 34: 01B101 1–10.
Miyake, M., Negishi, N., Izawa, M. et al. (2009). Effects of mask and necking deformation on bowing and twisting in high-aspect-... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Oh, Y.T., Kim, K.B., Shin, S.H. et al. (2018). Impact of etch angles on cell characteristics in 3D NAND flash memory. *Microelectron. J.* 79: 1–6.
Pargon, E., Martin, M., Thiault, J. et al. (2008). Linewidth roughness transfer measured by critical dimension atomic force microscopy during plasma patterning of polysilic... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Reynolds, G.W., Taylor, J.W., and Brooks, C.J. (1999). Direct measurement of X-ray mask sidewall roughness and its contribution to the overall sidewall roughness of chemically amplified resist features. *J. Vac. Sci. Technol., B* 17: 3420–3425.
Rudolph, U., Weikmann, E., Kinne, A. et al. (2004). Extending the capabili... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Sci. Technol., A 35: 01A102 1–6.
Shimmura, T., Suzuki, Y., Soda, S. et al. (2004). Mitigation of accumulated electric charge by deposited fluorocarbon film during SiO2 etching. *J. Vac. Sci. Technol., A* 22:
433–436.
Shin, H., Zhu, W., Donnelly, V.M., and Economou, D.J. (2012). Surprising importance of photo-assisted... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Vitale, S.A. and Smith, B.A. (2003). Reduction of silicon recess caused by plasma oxidation during high-density plasma polysilicon gate etching. *J. Vac. Sci. Technol., B* 21: 2205–2211.
Vitale, S.A., Chae, H., and Sawin, H.H. (2001). Silicon etching yields in F2, Cl2, Br2, and HBr high density plasmas. *J. Vac. Sci. ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
J. Appl. Phys. 108: 051101 1–20.
Yang, J.J., Strukov, D.B., and Stewart, D.R. (2013). Memristive devices for computing.
Nat. Nanotechnol. 8: 13–24.
Yashina, L.V., Püttner, R., Neudachina, V.S. et al. (2008). X-ray photoelectron studies of clean and oxidized α-GeTe(111) surfaces. *J. Appl. Phys.* 103: 094909 1–12.
Y... | text_only | 1_Atomic Layer Processing_semiconductor | ||
## 8.1 Mechanism And Performance Metrics Of Ion Beam Etching
IBE is a physical sputtering process and can be described by the mechanisms and equations 2.5, 2.6, 2.7, 2.8, and 2.9 in Section 2.5. The etching rate is a function of the ion flux, the sputtering yield, and the density of the material. The sputtering yield ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
To achieve vertical profiles, the wafer must be tilted and rotated. Without rotation, the profile will be asymmetric, which is typically not desired. The combined effect of tilting and rotation is that feature sidewalls that point toward the wafer edge are exposed to the plasma when they are closest to the ion source w... | text_only | 1_Atomic Layer Processing_semiconductor | ||
IBE is prone to aspect ratio dependent etching (ARDE) because the transport of the sputtered species out of the features is a function of their aspect ratio. The sputtered species are typically atoms and are nonvolatile because there is no chemistry involved in the process. They redeposit upon impact on feature sidewal... | text_only | 1_Atomic Layer Processing_semiconductor | ||
What makes the application of RIE to MRAM patterning even more challenging is that the tunneling dielectric, MgO, is very sensitive to chemical damage. The
| Element | Compound | Boiling point (∘C) |
|------------------------------------------------------------... | text_only | 1_Atomic Layer Processing_semiconductor | ||

use of halogens is not recommended for device performance reasons. Unless this requirement can be relaxed, this creates a large barrier for the use of RIE and ALE
technologies. In the absence of synergy from chemical reactions, a sputtering process must be used.
The angular depende... | text_only | 1_Atomic Layer Processing_semiconductor | ||
While new approaches must be found for patterning of high-density MRAM devices, IBE has established itself in the semiconductor industry as the preferred approach for embedded MRAM devices. The ability to change ion impact angles and to control the ion angular distribution and energy over a wide range is attractive for... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Altieri, N.D., Chen, J.K.C., and Chang, J.P. (2019). Controlling surface chemical states for selective patterning of CoFeB. *J. Vac. Sci. Technol., A* 37: 011303 1–6.
Chen, J.K.C., Altieri, N.D., Kim, T. et al. (2017). Directional etch of magnetic and noble metals. I. Role of surface oxidation states. *J. Vac. Sci. Te... | text_only | 1_Atomic Layer Processing_semiconductor | ||
# Etching Species Generation
In this chapter, we will establish a link between the etching mechanisms we studied so far and the various approaches to generate the reactive species needed to realize these etching processes.
The etching species used in thermal etching and thermal atomic layer etching
(ALE) are neutral ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
## 9.1 Introduction Of Low-Temperature Plasmas
A plasma is a quasi-neutral gaseous particle system in the form of free ions, electrons, and neutral particles. Why is plasma used in dry etching? This question seems a tautology since dry etching is frequently also called plasma etching. After plasma was discovered as th... | text_only | 1_Atomic Layer Processing_semiconductor | ||
RIE is implemented with a reactive plasma in direct contact with the wafer. This maximizes the species fluxes but also introduces enormous complexity. It makes RIE
a highly convoluted system with complicated surface mechanisms (see Eq. (7.4)) and strong feedback via the plasma. One of these feedback mechanisms is the r... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The density of neutral gas atoms, nn, is 2–6 orders of magnitude higher than the ion and electron density, ni and ne, respectively (Graves and Humbird 2002).
Other important parameters for typical nonequilibrium plasmas are listed in Table 9.1.
One defining characteristic of this type of plasma is that the charged sp... | text_only | 1_Atomic Layer Processing_semiconductor | ||
| Table 9.1 | Characteristics of nonequilibrium plasmas. |
|-----------------------------------------------------|----------------------------------------------|
| Characteristic property | Value |
| Gas press... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The pressure range for nonequilibrium plasmas is 1–1000 mTorr. The reason is that the mean free path of particles decreases for higher pressures. As the pressures increases, the probability of charged particle recombination raises. This is different for equilibrium plasmas where all particles, ion, electrons, and neutr... | text_only | 1_Atomic Layer Processing_semiconductor | ||

$$(9.1)$$
$$(9.2)$$
Figure 9.1 Electron energy distribution function (EEDF) for a nonequilibrium plasma.
Deviations from a Maxwellian distribution are common due to other effects in the plasma.
The energy of an electron is a function of its temperature, Te. The relationship for a... | text_only | 1_Atomic Layer Processing_semiconductor | ||
$$\mathbf{\partial}_{2}+\mathbf{\partial}$$
$${\bf\nabla}-{\bf O}^{*}+{\bf e}$$
$$(9.3)$$
$\mathbf{a}$ = $\mathbf{a}$
$\blacksquare$
O2 + e → O∗ + O∗ + e (9.3)
At higher electron energies, electron impact can also lead to ionization:
$$\mathrm{O}_{2}+\mathrm{e}\rightarrow\mathrm{O}_{2}^{+}+\mathrm{e}$$
$\eqref{eq:q_4}... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Large and complex ionic molecules can be formed via gentler electron attachment ionization. In this type of ionization, the electron is captured by the molecule to form a negative ion. For this ionization pathway, the electron energies must not exceed an energy of a few electron volts. If the energy is too high, electr... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Under the influence of the electric and magnetic fields, the neutral gas can be ionized and becomes conductive due to the free electrons in the gas. By passing currents through the gas, the charged species are heated, thereby sustaining the plasma. The peak neutral gas temperature can vary from near room temperature to... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The Debye length D is the parameter that defines the width of the shield and the voltage drop across it. It is the length over which the plasma shields itself from an applied electric field. The Debye length is a function of the electron density and temperature (Lieberman and Lichtenberg 2005):
$$\lambda_{D}=743\;{\sq... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The electron temperature also determines the sheath voltage Vsh (Lieberman and Lichtenberg 2005):
$$V_{\mathrm{sh}}={\frac{T_{e}}{2}}\ln\left({\frac{M_{i}}{2\Pi M_{e}}}\right)$$
$$(9.7)$$
)(9.7)
Here, Mi and Me are the mass of the ion and electron, respectively. For argon, Eq. (9.7) simplifies to (Lieberman and Lichte... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Another implication of Eq. (9.8) is that the sheath voltage cannot be zero. Ion masses are larger than the mass of an electron and the electron temperature must by larger than zero to sustain a plasma. This means that any plasma will lead to ion bombardment when being in contact with the wafer. Tools for application th... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Most plasma processes, however, require high-energy ions for etching. For these applications, the self-bias and hence electron temperature are not very important.
## 9.2 Capacitively Coupled Plasmas
Let us now study how RF power is coupled into the plasma and how this changes the electron temperature, sheath thicknes... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The plasma sheath acts like a capacitance. This allows to calculate the sheath voltage, which is induced by the RF signal (in addition to the self-bias we

(9.9) $\frac{}{}$
$$(9.10)$$
discussed previously):
$V_{\rm sb}=X_c I_c$
Vsh = XcI (9.9)
where Xc is the capacitive reactance... | text_only | 1_Atomic Layer Processing_semiconductor | ||
In most RIE tools, frequencies over 100 kHz are used and the ions are accelerated by VDC of a capacitive sheath. Resistive sheaths are interesting because they resemble the ion bombardment behavior of a plasma where the bias is pulsed. They are, however, not used in high-volume semiconductor production to date.
So far... | text_only | 1_Atomic Layer Processing_semiconductor | ||


0 50 100 150 200
This bimodal behavior for low frequencies has been modeled using particle-in-cell
(PIC) models (Kawamura et al. 1999). Simulations allow the investigation of a wide range of frequencies. The results, which are shown in Figure 9.6... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The IED for a gas mixture is the superposition for the IED of the ionic species.
If the gases are molecular, dissociation products have their own IED. This leads to IEDs with a series of peaks. Figure 9.8 depicts the measured IED for a capacitively coupled CF4 plasma, which exhibits peaks for the fragmentation product... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The frequency and mass dependence of the IED can be explained using the framework of an ion transient time i through the sheath (Kawamura et al. 1999):
i = 3dsh√Mi
∕2eVsh (9.12)
$$\overline{{{\mathrm{W_{s h}}}}}$$
$\mathbf{a}_i$ $\mathbf{a}_i$
Here, dsh is the sheath thickness, Mi is the ion mass, e is the elementary ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The other extreme case is i ≫ 1 where ions experience many sheath oscillations while traveling through the sheath. In this case, ions will respond to the time-averaged sheath potential, and the IED function will exhibit a single peak:
$$\Delta E_{i}\approx2V_{\mathrm{RF}}/\omega\tau_{i}$$
Ei ≈ 2VRF∕i (9.14)
Equation (... | text_only | 1_Atomic Layer Processing_semiconductor | ||
So far, we assumed that ions travel through the sheath without colliding with neutrals. This is not always the case. In nonequilibrium plasmas, the neutral density is several orders of magnitude higher than the ion and electron density.
These neutrals have the same density in the sheath as in the bulk plasma because t... | text_only | 1_Atomic Layer Processing_semiconductor | ||
$${\dot{\phi}}_{i}$$
i = 1Nn (9.15)
According to Eq. (9.15) the mean free path of an accelerated ion in the sheath is inversely proportional to the pressure. This is important to consider in process development. When a process engineer attempts to increase the process pressure to change the plasma chemistry, there is ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
$$\tau_{\mathrm{col}}=\lambda_{i}/V_{i}$$
∕Vi (9.16)
The existence of sheath collisions can be evaluated by comparing the ion transient time i and the collision time col. For i < col, the sheath is considered collision free.
Panagopoulos and Economou combined the concepts of ion transient time vs collision time and th... | text_only | 1_Atomic Layer Processing_semiconductor | ||
$$J_{i}=\frac{4}{9}\varepsilon_{0}\bigg(\frac{2e}{M_{i}}\bigg)^{1/2}\frac{V_{\mathrm{sh}}^{2/3}}{d^{2}}$$
d2 (9.17)
$$(9.18)$$
This law describes the space charge limited current in a plasma between planar walls or electrodes separated by a distance d. The existence of the sheath is caused by the difference in electro... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Next, we will discuss how the IED depends on the geometry of the etching reactor.
A capacitively coupled plasma has two electrodes that are characterized by their own capacitances. The equivalent circuit of a two-electrode RF plasma system is shown in Figure 9.12 (Koehler et al. 1985b). The capacitive sheath approxima... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The DC bias voltage VDC is related to the RF amplitude VRF by the expression
(Koehler et al. 1985b)
$$V_{\mathrm{DC}}=V_{\mathrm{RF}}\left({\frac{C_{\mathrm{ca}}-C_{w}}{C_{\mathrm{ca}}+C_{w}}}\right)$$
$$(9.22)$$
)(9.22)
Here,Cca andCw are the capacitances of the powered cathode and the grounded wall, respectively. T... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The gap between the cathode and the upper electrode (anode) is an important design parameter. In reactors with variable gap, it is also a process parameter. When the gap is increased, the anode to cathode ratio and the ion energy on the wafer increase while the ion energy on the upper electrode decreases. This is desir... | text_only | 1_Atomic Layer Processing_semiconductor | ||
In CCP reactors, both ion energy and flux are driven by capacitive coupling of RF
power. The simplest implementation of a CCP RIE reactor utilizes an RF-powered

cathode and grounded walls. The power that is applied to the cathode will sustain the plasma and accelerate the ions. The... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 9.16 depicts the corresponding electron densities. Here, the electron densities increase from 10 to 40 MHz and drop beyond 40 MHz. The data indicates that the driving frequency influences excitation of the plasma and impacts the electron and plasma density. This effect was brought to the attention of the plasma ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Furthermore, Flamm predicted that the RF frequency impacts the spatial distribution of species and electrical fields across the discharge, which means the plasma uniformity across the wafer can change. This is a very important point which limits the use of very high frequencies in etching if semiconductor devices (Flam... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Above 120 MHz, the increase appears to follow a frequency-squared dependence.
At the two highest frequencies investigated, 163 and 189 MHz, the authors found a shift in the spatial distribution from uniform to highly peaked in the center. Thus, the density inflection at approximately 100 MHz appears to be due to chang... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Most commercial CCP reactors utilize at least two frequencies, 13 MHz or lower to drive the ion energy and a high frequency (for example, 27 and 60 MHz) to drive the plasma density and ion flux. The use of such high frequencies effectively decouples to bias and source effects (Kitajima et al. 2000). The source frequenc... | text_only | 1_Atomic Layer Processing_semiconductor | ||

frequency RF components. Computational results by Shannon et al. are depicted in Figure 9.18. The graphs illustrate how the upper and lower energy peaks can be moved by changing the ratio of the lower and higher RF powers.
The mechanism that allows to change electron and plasma den... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Stochastic electron heating is the effect of energy transfer to electrons via the sheath. When electrons from the plasma reach the sheath, they get decelerated unless they are fast enough to escape to the electrode. As discussed before, the sheath moves with the RF frequency and the amplitude depends on the applied vol... | text_only | 1_Atomic Layer Processing_semiconductor | ||
In summary, the dependencies of the ion energy, IED, IAD, and ion flux on RF
power and frequency, ion mass, pressure, and electrode are complex and nonlinear.
Advanced CCP reactors utilize at least two RF frequencies to decouple ion energy and flux. For processes that use very high RF power, low frequency, and a mixtu... | text_only | 1_Atomic Layer Processing_semiconductor | ||

Electron current Ie Capacitive currents Other embodiments, for instance, helicon sources (Perry and Boswell 1989), are possible but are less frequently used in the manufacturing of semiconductor devices.
The driving force for the development of ICP/TCP sources was the need for proc... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Most ICP/TCP tools in the semiconductor industry use RF frequencies of 2 or 13.56 MHz. The RF frequency exceeds the electron collision frequency and the electron heating is determined the effective electric field underneath the dielectric window.
The power is absorbed by the plasma in a ring-shaped region. This leads ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
2000; Long et al. 2015). The uniformity can be further improved when the currents in the concentric coils are phase shifted (Banna et al. 2015). This concept can also be applied to three concentric coils (Banna et al. 2019).
The inductive coil also couples capacitively to the plasma. This can lead to sputtering of the... | text_only | 1_Atomic Layer Processing_semiconductor | ||
This has important implications for directional ALE, which requires ion energies of 50 eV and lower in the removal step. Both ICP/TCP reactors and CCP reactors with sufficiently high RF frequency (40 MHz and higher) can deliver such low ion energies under conditions when only the plasma source is powered. Of course, as... | text_only | 1_Atomic Layer Processing_semiconductor | ||



# 9.4 Ion Energy Distribution Modulation
The ion energy of both ICP/TCP and CCP reactors is driven by the bias power, which uses frequencies of 13.5 MHz and lower. Lower frequencies provide higher peak ion en... | text_only | 1_Atomic Layer Processing_semiconductor | ||
In this chapter, we will discuss solutions to narrow IEDs caused by capacitive coupling of RF power. Conceptually, such narrow IEDs can be stitched together to create the desired multi-peak IEDs in the time domain using plasma pulsing. We will investigate plasma pulsing in Section 9.5.
The fundamental reason why IEDs ... | text_only | 1_Atomic Layer Processing_semiconductor | ||

a narrow IED. Short high-voltage pulses are needed to prevent charge accumulation on the substrate surface (Wang and Wendt 2000). To produce a constant sheath potential, the voltage at the cathode must be ramped to compensate for charging.
The signal to the cathode is produced by a... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The right panel of Figure 9.22 illustrates that bimodal IEDs with two distinct peaks can be produced using the TWB approach. Here, the RF signal has two levels of

negative potential. The relative duration of the two levels determines the relative flux of the high- and low-energy io... | text_only | 1_Atomic Layer Processing_semiconductor | ||
The authors found that the silicon oxide to silicon selectivity in fluorocarbon plasmas can be controlled by adjusting the width and energy of the IED via tuning of the short positive voltage pulse. Tailoring of the bias waveform allows tuning the average ion energy and the width of the IED to fit the process window. T... | text_only | 1_Atomic Layer Processing_semiconductor | ||
For pulsing frequencies in the kilohertz range, the duration of these steps is in the order of several milliseconds. Because gases cannot be exchanged that fast, the changes in plasma chemistry can come only from variations of the electron temperature and dissociation pattern when the source power is pulsed. The fundam... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Plasma pulsing goes beyond simply turning on and off the source and bias power when considering the transitions between steps (Midha and Economou 2000). New conditions such as ion–ion plasmas (IIPs) can be produced in these

Dual level bias / single level TWB Single level bias / dua... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Figure 9.25 shows the evolution of species wall fluxes predicted by a model of pulsed chlorine plasma between two parallel plates (Midha and Economou 2000).
Each cycle is separated into four time segments: (1) early active glow, (2) late active glow, (3) early afterglow, and (4) late afterglow. The simulations show a ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
This means source pulsing produces a bimodal ion energy distribution with the high energy being the self-bias of the active glow and the low energy corresponding to an IIP in the afterglow. The ratio between the low- and high-energy peaks is determined by the duty cycle as shown in Figure 9.26. Thus, source pulsing off... | text_only | 1_Atomic Layer Processing_semiconductor | ||

Figure 9.26 Ion energy distribution functions in an argon microwave plasma with a peak power of 960 W
pulsed at 1 kHz for varying duty cycles. Source:
Zabeida and Martinu (1999). © 1999 AIP Publishing.

IEDs but also reduce the ion flux, which ma... | text_only | 1_Atomic Layer Processing_semiconductor | ||
## 9.6 Grid Sources
Ion beam etching (IBE) and radical etching are examples of technologies adjacent to RIE, which cover specialized, all chemical (see Chapter 5) or all physical etching (see Chapter 8). IBE and radical etch reactors can be viewed as derivatives of RIE reactors where some of the species are being supp... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Advanced IBE sources use a three-grid design to allow for acceleration of the beamlets, which are formed in each of the several hundred openings in the grid.
A schematic of such a source is depicted in Figure 9.29. The first grid sets the acceleration voltage and is called the plasma electrode. The second grid and the... | text_only | 1_Atomic Layer Processing_semiconductor | ||


An in-depth review of ion beam sources can be found in "The physics and technology of ion sources" edited by Brown (2004).
The grid in radical etching reactors is there to block the ions from impinging onto the wafer. In the simplest case, both ... | text_only | 1_Atomic Layer Processing_semiconductor | ||
Grids have been combined with plasma pulsing of a capacitively coupled plasma to extract nearly monoenergetic ion beams. During the pulsing, the electron temperature decays in the afterglow, resulting in nearly uniform plasma potential and minimal energy spread of ions. The ion energy was controlled by a DC bias on an ... | text_only | 1_Atomic Layer Processing_semiconductor |
Subsets and Splits
No community queries yet